General
Property | Value | Temperature |
---|---|---|
Density | 2.68 - 2.69 g/cm³ Show Material materials with Density of 2.68 - 2.69 g/cm³ at 23.0 °C | 23.0 °C |
Mechanical
Property | Value | Temperature | Comment |
---|---|---|---|
Bending angle 180° | 0 - 0.5 °/t Show Material materials with Bending angle 180° of 0 - 0.5 °/t at 23.0 °C | 23.0 °C | |
Bending angle 90° | 0 - 2 °/t Show Material materials with Bending angle 90° of 0 - 2 °/t at 23.0 °C | 23.0 °C | |
Elastic modulus | 69 - 70 GPa Show Material materials with Elastic modulus of 69 - 70 GPa at 23.0 °C | 23.0 °C | |
Elongation | 20 % Show Material materials with Elongation of 20 % at 20.0 °C | 20.0 °C | |
Elongation A100 | 20 % Show Material materials with Elongation A100 of 20 % at 23.0 °C | 23.0 °C | |
Elongation A50 | 16 - 21 % Show Material materials with Elongation A50 of 16 - 21 % at 20.0 °C | 20.0 °C | |
16 - 21 % Show Material materials with Elongation A50 of 16 - 21 % at 23.0 °C | 23.0 °C | ||
Elongation A50, transverse | 16 - 21 % Show Material materials with Elongation A50, transverse of 16 - 21 % at 20.0 °C | 20.0 °C | |
Elongation, transverse | 20 % Show Material materials with Elongation, transverse of 20 % at 20.0 °C | 20.0 °C | |
Hardness, Brinell | 36 [-] Show Material materials with Hardness, Brinell of 36 [-] at 20.0 °C | 20.0 °C | |
36 [-] Show Material materials with Hardness, Brinell of 36 [-] at 23.0 °C | 23.0 °C | ||
Plane-Strain Fracture Toughnes | 22 - 35 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Shear modulus | 26 - 26.5 GPa Show Material materials with Shear modulus of 26 - 26.5 GPa at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Tensile strength | 130 - 170 MPa Show Material materials with Tensile strength of 130 - 170 MPa at 20.0 °C | 20.0 °C | |
130 - 170 MPa Show Material materials with Tensile strength of 130 - 170 MPa at 23.0 °C | 23.0 °C | ||
Tensile strength, transverse | 130 - 170 MPa Show Material materials with Tensile strength, transverse of 130 - 170 MPa at 20.0 °C | 20.0 °C | |
Yield strength Rp0.2 | 45 MPa Show Material materials with Yield strength Rp0.2 of 45 MPa at 20.0 °C | 20.0 °C | |
45 MPa Show Material materials with Yield strength Rp0.2 of 45 MPa at 23.0 °C | 23.0 °C | ||
Yield strength Rp0.2, transverse | 45 MPa Show Material materials with Yield strength Rp0.2, transverse of 45 MPa at 20.0 °C | 20.0 °C |
Thermal
Property | Value | Temperature | Comment |
---|---|---|---|
Coefficient of thermal expansion | 2.38E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.38E-5 1/K at 20.0 °C | 20.0 °C | |
2.38E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.38E-5 1/K at 100.0 °C | 100.0 °C | ||
Max service temperature | 150 °C Show Material materials with Max service temperature of 150 °C | Typical for Wrought 5000 Series Aluminium | |
Melting point | 620 - 650 °C Show Material materials with Melting point of 620 - 650 °C | ||
Specific heat capacity | 879 - 963 J/(kg·K) Show Material materials with Specific heat capacity of 879 - 963 J/(kg·K) at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Thermal conductivity | 170 - 193 W/(m·K) Show Material materials with Thermal conductivity of 170 - 193 W/(m·K) at 23.0 °C | 23.0 °C |
Electrical
Property | Value | Temperature |
---|---|---|
Electrical conductivity | 2.30E+7 - 2.90E+7 S/m Show Material materials with Electrical conductivity of 2.30E+7 - 2.90E+7 S/m at 23.0 °C | 23.0 °C |
Electrical resistivity | 3.45E-8 - 4.35E-8 Ω·m Show Material materials with Electrical resistivity of 3.45E-8 - 4.35E-8 Ω·m at 23.0 °C | 23.0 °C |
Chemical properties
Property | ||
---|---|---|
Chromium | 0.1 % | |
Copper | 0.2 % | |
Iron | 0.7 % | |
Magnesium | 1.1 - 1.8 % | |
Manganese | 0.1 - 0.3 % | |
Other | each 0.05, total 0.10, Rest Al | |
Silicon | 0.4 % | |
Zinc | 0.25 % |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |