Material EN AW-Al Mg1(B) is produced for wire and prewire for mechanical applications, for extruded and drawn components. The material is food-safe. To the comparable mark AlMg1,8, material No. 3.3326 acc. to DIN 1725-1 : 1983-02, applies: The alloy has a high resistance to corrosion, seawater and salted atmosphere. Strength increases and cold workability decreases according to the Mg-content. It is naturally hard, i.e. a strength increase can only be achieved by cold forming, not by controlled heat treatment. It is ideal for brightening and anodizing. Machinability and weldability are enhanced by increasing Mg-content. The mark AlMg1,8 as a AlMg-alloy shows a relatively low strength. Application: ferrules for wire cables, in engineering for load-carrying constructions and for transport containers. In electrical engineering for aerials and parabolic mirrors.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueTemperature

Density

2.68 g/cm³

Show Material materials with Density of 2.68 g/cm³ at 20.0 °C

20.0 °C

2.69 g/cm³

Show Material materials with Density of 2.69 g/cm³ at 23.0 °C

23.0 °C

Mechanical

PropertyValueTemperatureComment

Elastic modulus

70 GPa

Show Material materials with Elastic modulus of 70 GPa at 23.0 °C

23.0 °C

Elongation

16 %

Show Material materials with Elongation of 16 % at 20.0 °C

20.0 °C

Elongation A100

16 %

Show Material materials with Elongation A100 of 16 % at 23.0 °C

23.0 °C

Elongation A50

14 %

Show Material materials with Elongation A50 of 14 % at 20.0 °C

20.0 °C

14 %

Show Material materials with Elongation A50 of 14 % at 23.0 °C

23.0 °C

Unlock all property charts

Hardness, Brinell

40 [-]

Show Material materials with Hardness, Brinell of 40 [-] at 20.0 °C

20.0 °C

Plane-Strain Fracture Toughnes

22 - 35 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m at 23.0 °C

23.0 °C

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-] at 23.0 °C

23.0 °C

Typical for Wrought 5000 Series Aluminium

Shear modulus

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa at 20.0 °C

20.0 °C

Tensile strength

150 MPa

Show Material materials with Tensile strength of 150 MPa at 20.0 °C

20.0 °C

150 MPa

Show Material materials with Tensile strength of 150 MPa at 23.0 °C

23.0 °C

Unlock all property charts

Yield strength Rp0.2

50 - 60 MPa

Show Material materials with Yield strength Rp0.2 of 50 - 60 MPa at 20.0 °C

20.0 °C

50 - 60 MPa

Show Material materials with Yield strength Rp0.2 of 50 - 60 MPa at 23.0 °C

23.0 °C

Unlock all property charts

Thermal

PropertyValueTemperatureComment

Coefficient of thermal expansion

2.38E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.38E-5 1/K at 20.0 °C

20.0 °C

2.38E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.38E-5 1/K at 100.0 °C

100.0 °C

Unlock all property charts

Max service temperature

150 °C

Show Material materials with Max service temperature of 150 °C

Typical for Wrought 5000 Series Aluminium

Melting point

560 - 655 °C

Show Material materials with Melting point of 560 - 655 °C

Typical for Wrought 5000 Series Aluminium

Specific heat capacity

921 J/(kg·K)

Show Material materials with Specific heat capacity of 921 J/(kg·K) at 20.0 °C

20.0 °C

Thermal conductivity

135 - 167 W/(m·K)

Show Material materials with Thermal conductivity of 135 - 167 W/(m·K) at 20.0 °C

20.0 °C

Electrical

PropertyValueTemperatureComment

Electrical conductivity

2.20E+7 - 2.60E+7 S/m

Show Material materials with Electrical conductivity of 2.20E+7 - 2.60E+7 S/m at 20.0 °C

20.0 °C

Electrical resistivity

3.3E-8 - 5E-8 Ω·m

Show Material materials with Electrical resistivity of 3.3E-8 - 5E-8 Ω·m at 23.0 °C

23.0 °C

Typical for Wrought 5000 Series Aluminium

Chemical properties

Property

Chromium

0.3 %

Copper

0.05 %

Iron

0.45 %

Magnesium

1.4 - 2.1 %

Manganese

0.25 %

Other

each 0.05, total 0.15, Rest Al

Silicon

0.3 %

Titanium

0.1 %

Zinc

0.2 %

Technological properties

Property
Anodizing

decorative: sufficient, Protective: very good

Brazing

hard brazing (with flux/ without flux): ausreichend - ungeeignet / mangelhaft, friction soldering: good, soft brazing with flux: sufficient

Corrosion properties

Seawater: good, weathering: very good

Workability

Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / acceptable (H12)