EN 573-3 Grade AW-5052 H111

Want to keep this datasheet? Save it now in your required format

Description

Aluminum EN AW-5052 is a non-heat treatable alloy with excellent finishing qualities. EN AW-5052 offers better corrosion resistance than most aluminum alloys, especially to salt water and marine atmospheres. This alloy can be readily welded using most common techniques and is in fact offers some of the best welding characteristics of all aluminum alloys.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey,Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.68 g/cm³

Show Material materials with Density of 2.68 g/cm³

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

2.68 g/cm³

Show Material materials with Density of 2.68 g/cm³

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 573-3

Sheet, Rod, Flat, Tube

20.0 °C

2.68 - 2.69 g/cm³

Show Material materials with Density of 2.68 - 2.69 g/cm³

H111

EN 573-3

Rod, Flat, Tube

20.0 °C

2.69 g/cm³

Show Material materials with Density of 2.69 g/cm³

H111

EN 573-3

Rod, Flat, Tube

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.2 mm

Show Material materials with Thickness of 0.2 mm

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

0.2 mm

Sheet

6.0 mm

Show Material materials with Thickness of 6.0 mm

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

6.0 mm

Sheet

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending angle 180°

0 °/t

Show Material materials with Bending angle 180° of 0 °/t

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

0.5 °/t

Show Material materials with Bending angle 180° of 0.5 °/t

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

Bending angle 90°

0 °/t

Show Material materials with Bending angle 90° of 0 °/t

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

2.0 °/t

Show Material materials with Bending angle 90° of 2.0 °/t

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

Elastic modulus

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 573-3

Sheet, Rod, Flat, Tube

Elongation

12.0 %

Show Material materials with Elongation of 12.0 %

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

12 %

Show Material materials with Elongation of 12 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

A50

14.0 %

Show Material materials with Elongation of 14.0 %

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

15.0 %

Show Material materials with Elongation of 15.0 %

H111

EN 573-3, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

16.0 %

Show Material materials with Elongation of 16.0 %

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

17.0 %

Show Material materials with Elongation of 17.0 %

H111

EN 573-3, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

17.0 %

Show Material materials with Elongation of 17.0 %

H111

EN 573-3, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A100

18.0 %

Show Material materials with Elongation of 18.0 %

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

18.0 %

Show Material materials with Elongation of 18.0 %

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A100

19.0 %

Show Material materials with Elongation of 19.0 %

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

20.0 %

Show Material materials with Elongation of 20.0 %

H111

EN 573-3, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A100

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

H111

EN 573-3

Flat

A50

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

H111

EN 573-3

Flat

A50 Transverse

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

H111

EN 573-3

Flat

A50

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

H111

EN 573-3

Flat

A50 Transverse

20.0 °C

15.0 %

Show Material materials with Elongation of 15.0 %

H111

EN 573-3

Rod, Tube

A50

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

H111

EN 573-3

Flat

A50

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

H111

EN 573-3

Flat

A50 Transverse

20.0 °C

17.0 %

Show Material materials with Elongation of 17.0 %

H111

EN 573-3

Rod, Tube

A50

20.0 °C

17.0 %

Show Material materials with Elongation of 17.0 %

H111

EN 573-3

Rod, Tube

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

H111

EN 573-3

Flat

A50

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

H111

EN 573-3

Flat

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

H111

EN 573-3

Flat

A50 Transverse

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

H111

EN 573-3

Flat

Transverse

20.0 °C

19.0 %

Show Material materials with Elongation of 19.0 %

H111

EN 573-3

Flat

A50

20.0 °C

19.0 %

Show Material materials with Elongation of 19.0 %

H111

EN 573-3

Flat

A50 Transverse

20.0 °C

20.0 %

Show Material materials with Elongation of 20.0 %

H111

EN 573-3

Rod, Tube

Hardness, Brinell

46.0 [-]

Show Material materials with Hardness, Brinell of 46.0 [-]

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

47.0 [-]

Show Material materials with Hardness, Brinell of 47.0 [-]

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

45.0 [-]

Show Material materials with Hardness, Brinell of 45.0 [-]

H111

EN 573-3

Rod, Tube

20.0 °C

46.0 - 47.0 [-]

Show Material materials with Hardness, Brinell of 46.0 - 47.0 [-]

H111

EN 573-3

Flat

20.0 °C

46.0 [-]

Show Material materials with Hardness, Brinell of 46.0 [-]

H111

EN 573-3

Flat

20.0 °C

47.0 [-]

Show Material materials with Hardness, Brinell of 47.0 [-]

H111

EN 573-3

Rod, Tube, Flat

Hardness, HBW

47 [-]

Show Material materials with Hardness, HBW of 47 [-]

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

H111

EN 573-3

Rod, Flat, Tube

Shear modulus

26.3 GPa

Show Material materials with Shear modulus of 26.3 GPa

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

20.0 °C

26.3 - 27.0 GPa

Show Material materials with Shear modulus of 26.3 - 27.0 GPa

H111

EN 573-3

Rod, Flat, Tube

20.0 °C

26.3 GPa

Show Material materials with Shear modulus of 26.3 GPa

H111

EN 573-3

Rod, Flat, Tube

Tensile strength

20.0 °C

165.0 - 215.0 MPa

Show Material materials with Tensile strength of 165.0 - 215.0 MPa

H111

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

165.0 - 215.0 MPa

Show Material materials with Tensile strength of 165.0 - 215.0 MPa

H111

EN 573-3

Flat

Transverse

20.0 °C

170.0 MPa

Show Material materials with Tensile strength of 170.0 MPa

H111

EN 573-3

Rod

20.0 °C

170.0 - 230.0 MPa

Show Material materials with Tensile strength of 170.0 - 230.0 MPa

H111

EN 573-3, EN 754, EN 755

Rod, Tube, Strip, Sheet, Plate, Foil, Wire, Bar

20.0 °C

170.0 - 215.0 MPa

Show Material materials with Tensile strength of 170.0 - 215.0 MPa

H111

EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Flat, Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

170.0 - 215.0 MPa

Show Material materials with Tensile strength of 170.0 - 215.0 MPa

H111

EN 573-3

Flat

Transverse

Yield strength

65.0 MPa

Show Material materials with Yield strength of 65.0 MPa

H111

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

RP02

65 MPa

Show Material materials with Yield strength of 65 MPa

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

70.0 MPa

Show Material materials with Yield strength of 70.0 MPa

H111

EN 573-3, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

RP02

20.0 °C

65.0 MPa

Show Material materials with Yield strength of 65.0 MPa

H111

EN 573-3

Rod, Tube, Flat

RP02

20.0 °C

65.0 MPa

Show Material materials with Yield strength of 65.0 MPa

H111

EN 573-3

Flat

RP02 Transverse

20.0 °C

70.0 MPa

Show Material materials with Yield strength of 70.0 MPa

H111

EN 573-3

Rod, Tube

RP02

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

-50.0 °C

2.21e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.21e-05 1/K

H111

EN 573-3

Rod, Flat, Tube

-50 °C

2.2100000000000002e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2100000000000002e-05 1/K

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20 °C

2.2100000000000002e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2100000000000002e-05 1/K

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat

20 °C

2.48e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.48e-05 1/K

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat

20 °C

2.5699999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5699999999999998e-05 1/K

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

100 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat

100.0 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

20-100°C

200 °C

2.48e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.48e-05 1/K

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat

200.0 °C

2.48e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.48e-05 1/K

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat

300 °C

2.5699999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5699999999999998e-05 1/K

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

300.0 °C

2.57e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.57e-05 1/K

H111

EN 573-3

Rod, Flat, Tube

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

605.0 - 650.0 °C

Show Material materials with Melting point of 605.0 - 650.0 °C

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

607.0 - 649.0 °C

Show Material materials with Melting point of 607.0 - 649.0 °C

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

Specific heat capacity

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

H111

EN 573-3

Rod, Flat, Tube

20.0 °C

900.0 - 901.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 - 901.0 J/(kg·K)

H111

EN 573-3

Rod, Flat, Tube

20.0 °C

901.0 J/(kg·K)

Show Material materials with Specific heat capacity of 901.0 J/(kg·K)

H111

EN 573-3

Rod, Flat, Tube

Thermal conductivity

138 W/(m·K)

Show Material materials with Thermal conductivity of 138 W/(m·K)

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

130.0 - 150.0 W/(m·K)

Show Material materials with Thermal conductivity of 130.0 - 150.0 W/(m·K)

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat

20.0 °C

130.0 - 138.0 W/(m·K)

Show Material materials with Thermal conductivity of 130.0 - 138.0 W/(m·K)

H111

EN 573-3

Rod, Flat, Tube

20.0 °C

138.0 - 150.0 W/(m·K)

Show Material materials with Thermal conductivity of 138.0 - 150.0 W/(m·K)

H111

EN 573-3

Rod, Flat, Tube

20.0 °C

138.0 W/(m·K)

Show Material materials with Thermal conductivity of 138.0 W/(m·K)

H111

EN 573-3

Rod, Flat, Tube

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20000000.0 S/m

Show Material materials with Electrical conductivity of 20000000.0 S/m

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

19000000.0 - 21000000.0 S/m

Show Material materials with Electrical conductivity of 19000000.0 - 21000000.0 S/m

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat

Electrical resistivity

4.76e-08 - 5.26e-08 Ω·m

Show Material materials with Electrical resistivity of 4.76e-08 - 5.26e-08 Ω·m

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

4.9e-08 Ω·m

Show Material materials with Electrical resistivity of 4.9e-08 Ω·m

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

5e-08 Ω·m

Show Material materials with Electrical resistivity of 5e-08 Ω·m

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

4.7e-08 - 4.95e-08 Ω·m

Show Material materials with Electrical resistivity of 4.7e-08 - 4.95e-08 Ω·m

H111

EN 573-3

Rod, Flat, Tube

20.0 °C

4.7e-08 - 5.2e-08 Ω·m

Show Material materials with Electrical resistivity of 4.7e-08 - 5.2e-08 Ω·m

H111

EN 573-3

Rod, Flat, Tube

20.0 °C

4.95e-08 Ω·m

Show Material materials with Electrical resistivity of 4.95e-08 Ω·m

H111

EN 573-3

Rod, Flat, Tube

20.0 °C

4.95e-08 - 5.2e-08 Ω·m

Show Material materials with Electrical resistivity of 4.95e-08 - 5.2e-08 Ω·m

H111

EN 573-3

Rod, Flat, Tube

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.15 - 0.35 %

Show Material materials with Chromium of 0.15 - 0.35 %

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Wire, Bar

Copper

0.1 %

Show Material materials with Copper of 0.1 %

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Wire, Bar

0.1 %

Show Material materials with Copper of 0.1 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

Iron

0.4 %

Show Material materials with Iron of 0.4 %

H111

EN 573-3

Rod, Flat, Tube

0.40 %

Show Material materials with Iron of 0.40 %

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

0.4 %

Show Material materials with Iron of 0.4 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

Magnesium

2.2 - 2.8 %

Show Material materials with Magnesium of 2.2 - 2.8 %

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Wire, Bar

Manganese

0.1 %

Show Material materials with Manganese of 0.1 %

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Wire, Bar

0.1 %

Show Material materials with Manganese of 0.1 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

Other

0.15 %

Show Material materials with Other of 0.15 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

Silicon

0.25 %

Show Material materials with Silicon of 0.25 %

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Wire, Bar

0.25 %

Show Material materials with Silicon of 0.25 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

Zinc

0.1 %

Show Material materials with Zinc of 0.1 %

H111

EN 573-3, EN 485, EN 13195, EN 754, EN 755

Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Wire, Bar

0.1 %

Show Material materials with Zinc of 0.1 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

Technological properties

Property
Anodizing

decorative: good, Protective: very good

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing quality; Electronic devices: Housing devices; Closures: Easy open; Food can: Body, Lids; Components: Heat shields, Access hatches, Spoilers, General trasportation

Corrosion properties

Seawater: very good to good, weathering: good

Welding

Very Good

Workability

Bending / Spinning (cold): very good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / good (H12)