EN 573-3 Grade AW-5052 H12

Want to keep this datasheet? Save it now in your required format

Description

Aluminum EN AW-5052 is a non-heat treatable alloy with excellent finishing qualities. EN AW-5052 offers better corrosion resistance than most aluminum alloys, especially to salt water and marine atmospheres. This alloy can be readily welded using most common techniques and is in fact offers some of the best welding characteristics of all aluminum alloys.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey,Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.68 g/cm³

Show Material materials with Density of 2.68 g/cm³

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

2.68 g/cm³

Show Material materials with Density of 2.68 g/cm³

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 573-3

Sheet, Rod, Flat

20.0 °C

2.68 - 2.69 g/cm³

Show Material materials with Density of 2.68 - 2.69 g/cm³

H12

EN 573-3

Rod, Flat

20.0 °C

2.69 g/cm³

Show Material materials with Density of 2.69 g/cm³

H12

EN 573-3

Rod, Flat

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.2 mm

Show Material materials with Thickness of 0.2 mm

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

0.2 mm

Sheet

6.0 mm

Show Material materials with Thickness of 6.0 mm

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

6.0 mm

Sheet

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

110.0 MPa

Show Material materials with Bending Fatigue Strength of 110.0 MPa

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

Elastic modulus

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 573-3

Sheet, Rod, Flat

Elongation

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H12

EN 573-3

Rod, Flat

A50

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

H12

EN 573-3

Flat

A50

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

H12

EN 573-3

Flat

A50

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

H12

EN 573-3

Flat

A50

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

H12

EN 573-3

Flat

A50

4.0 %

Show Material materials with Elongation of 4.0 %

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

10.0 %

Show Material materials with Elongation of 10.0 %

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

8.0 %

Show Material materials with Elongation of 8.0 %

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

6.0 %

Show Material materials with Elongation of 6.0 %

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

5.0 %

Show Material materials with Elongation of 5.0 %

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

4 %

Show Material materials with Elongation of 4 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

A50

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

H12

EN 573-3

Rod

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

H12

EN 573-3

Flat

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

H12

EN 573-3

Flat

A50 Transverse

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H12

EN 573-3

Flat

A50 Transverse

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

H12

EN 573-3

Flat

A50 Transverse

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

H12

EN 573-3

Flat

A50 Transverse

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

H12

EN 573-3

Flat

A50 Transverse

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

H12

EN 573-3

Flat

Transverse

9.0 %

Show Material materials with Elongation of 9.0 %

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A100

7.0 %

Show Material materials with Elongation of 7.0 %

H12

EN 573-3, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A100

Unlock all property charts

Hardness, Brinell

20.0 °C

60.0 [-]

Show Material materials with Hardness, Brinell of 60.0 [-]

H12

EN 573-3

Rod

20.0 °C

63.0 [-]

Show Material materials with Hardness, Brinell of 63.0 [-]

H12

EN 573-3

Flat

63.0 [-]

Show Material materials with Hardness, Brinell of 63.0 [-]

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

Unlock all property charts

Hardness, HBW

63 [-]

Show Material materials with Hardness, HBW of 63 [-]

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

H12

EN 573-3

Rod, Flat

Shear modulus

26.3 GPa

Show Material materials with Shear modulus of 26.3 GPa

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

20.0 °C

26.3 - 27.0 GPa

Show Material materials with Shear modulus of 26.3 - 27.0 GPa

H12

EN 573-3

Rod, Flat

20.0 °C

26.3 GPa

Show Material materials with Shear modulus of 26.3 GPa

H12

EN 573-3

Rod, Flat

Unlock all property charts

Tensile strength

20.0 °C

210.0 - 250.0 MPa

Show Material materials with Tensile strength of 210.0 - 250.0 MPa

H12

EN 573-3, EN 754

Rod, Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

210.0 - 260.0 MPa

Show Material materials with Tensile strength of 210.0 - 260.0 MPa

H12

EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Flat, Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

210.0 - 260.0 MPa

Show Material materials with Tensile strength of 210.0 - 260.0 MPa

H12

EN 573-3

Flat

Transverse

Unlock all property charts

Yield strength

20.0 °C

160.0 MPa

Show Material materials with Yield strength of 160.0 MPa

H12

EN 573-3

Rod, Flat

RP02

160.0 MPa

Show Material materials with Yield strength of 160.0 MPa

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

RP02

20.0 °C

160.0 MPa

Show Material materials with Yield strength of 160.0 MPa

H12

EN 573-3

Flat

RP02 Transverse

160 MPa

Show Material materials with Yield strength of 160 MPa

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

Unlock all property charts

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

20-100°C

100 °C, 20 °C, 100.0 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat

300 °C, 20 °C

2.5699999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5699999999999998e-05 1/K

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

200 °C, 20 °C, 200.0 °C

2.48e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.48e-05 1/K

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat

20 °C, -50 °C

2.2100000000000002e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2100000000000002e-05 1/K

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

-50.0 °C

2.21e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.21e-05 1/K

H12

EN 573-3

Rod, Flat

300.0 °C

2.57e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.57e-05 1/K

H12

EN 573-3

Rod, Flat

Unlock all property charts

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

605.0 - 650.0 °C

Show Material materials with Melting point of 605.0 - 650.0 °C

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

607.0 - 649.0 °C

Show Material materials with Melting point of 607.0 - 649.0 °C

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

Specific heat capacity

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

H12

EN 573-3

Rod, Flat

20.0 °C

900.0 - 901.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 - 901.0 J/(kg·K)

H12

EN 573-3

Rod, Flat

20.0 °C

901.0 J/(kg·K)

Show Material materials with Specific heat capacity of 901.0 J/(kg·K)

H12

EN 573-3

Rod, Flat

Unlock all property charts

Thermal conductivity

138 W/(m·K)

Show Material materials with Thermal conductivity of 138 W/(m·K)

H12

EN 573-3, EN 485, EN 754, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

130.0 - 150.0 W/(m·K)

Show Material materials with Thermal conductivity of 130.0 - 150.0 W/(m·K)

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat

20.0 °C

138.0 - 150.0 W/(m·K)

Show Material materials with Thermal conductivity of 138.0 - 150.0 W/(m·K)

H12

EN 573-3

Rod, Flat

20.0 °C

138.0 W/(m·K)

Show Material materials with Thermal conductivity of 138.0 W/(m·K)

H12

EN 573-3

Rod, Flat

20.0 °C

130.0 - 138.0 W/(m·K)

Show Material materials with Thermal conductivity of 130.0 - 138.0 W/(m·K)

H12

EN 573-3

Rod, Flat

Unlock all property charts

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20000000.0 S/m

Show Material materials with Electrical conductivity of 20000000.0 S/m

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

19000000.0 - 21000000.0 S/m

Show Material materials with Electrical conductivity of 19000000.0 - 21000000.0 S/m

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat

Electrical resistivity

5e-08 Ω·m

Show Material materials with Electrical resistivity of 5e-08 Ω·m

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

4.76e-08 - 5.26e-08 Ω·m

Show Material materials with Electrical resistivity of 4.76e-08 - 5.26e-08 Ω·m

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

4.9e-08 Ω·m

Show Material materials with Electrical resistivity of 4.9e-08 Ω·m

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

20.0 °C

4.95e-08 Ω·m

Show Material materials with Electrical resistivity of 4.95e-08 Ω·m

H12

EN 573-3

Rod, Flat

20.0 °C

4.7e-08 - 4.95e-08 Ω·m

Show Material materials with Electrical resistivity of 4.7e-08 - 4.95e-08 Ω·m

H12

EN 573-3

Rod, Flat

20.0 °C

4.95e-08 - 5.2e-08 Ω·m

Show Material materials with Electrical resistivity of 4.95e-08 - 5.2e-08 Ω·m

H12

EN 573-3

Rod, Flat

20.0 °C

4.7e-08 - 5.2e-08 Ω·m

Show Material materials with Electrical resistivity of 4.7e-08 - 5.2e-08 Ω·m

H12

EN 573-3

Rod, Flat

Unlock all property charts

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.15 - 0.35 %

Show Material materials with Chromium of 0.15 - 0.35 %

H12

EN 573-3, EN 485, EN 754, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Rod, Flat, Strip, Sheet, Plate, Foil, Wire, Tube, Bar

Copper

0.1 %

Show Material materials with Copper of 0.1 %

H12

EN 573-3, EN 485, EN 754

Rod, Flat, Strip, Sheet, Plate, Foil, Wire, Tube, Bar

0.1 %

Show Material materials with Copper of 0.1 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

Iron

0.4 %

Show Material materials with Iron of 0.4 %

H12

EN 573-3

Rod, Flat

0.40 %

Show Material materials with Iron of 0.40 %

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

0.4 %

Show Material materials with Iron of 0.4 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

Magnesium

2.2 - 2.8 %

Show Material materials with Magnesium of 2.2 - 2.8 %

H12

EN 573-3, EN 485, EN 754, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Rod, Flat, Strip, Sheet, Plate, Foil, Wire, Tube, Bar

Manganese

0.1 %

Show Material materials with Manganese of 0.1 %

H12

EN 573-3, EN 485, EN 754

Rod, Flat, Strip, Sheet, Plate, Foil, Wire, Tube, Bar

0.1 %

Show Material materials with Manganese of 0.1 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

Other

0.15 %

Show Material materials with Other of 0.15 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

Silicon

0.25 %

Show Material materials with Silicon of 0.25 %

H12

EN 573-3, EN 485, EN 754

Rod, Flat, Strip, Sheet, Plate, Foil, Wire, Tube, Bar

0.25 %

Show Material materials with Silicon of 0.25 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

Zinc

0.1 %

Show Material materials with Zinc of 0.1 %

H12

EN 573-3, EN 485, EN 754

Rod, Flat, Strip, Sheet, Plate, Foil, Wire, Tube, Bar

0.1 %

Show Material materials with Zinc of 0.1 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet

Technological properties

Property
Anodizing

decorative: good, Protective: very good

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing quality; Electronic devices: Housing devices; Closures: Easy open; Food can: Body, Lids; Components: Heat shields, Access hatches, Spoilers, General trasportation

Corrosion properties

Seawater: very good to good, weathering: good

Welding

Very Good

Workability