General
Property | Value | Temperature |
---|---|---|
Density | 2.7 g/cm³ Show Material materials with Density of 2.7 g/cm³ at 20.0 °C | 20.0 °C |
2.69 - 2.7 g/cm³ Show Material materials with Density of 2.69 - 2.7 g/cm³ at 23.0 °C | 23.0 °C | |
Dimension
Property | Value |
---|---|
Thickness | 0.2 - 3 mm Show Material materials with Thickness of 0.2 - 3 mm |
Mechanical
Property | Value | Temperature | Comment |
---|---|---|---|
Bending angle 90° | 0.5 - 1 °/t Show Material materials with Bending angle 90° of 0.5 - 1 °/t at 23.0 °C | 23.0 °C | according to EN 485-2 |
Elastic modulus | 70 GPa Show Material materials with Elastic modulus of 70 GPa at -270.0 °C | -270.0 °C | |
60 - 70 GPa Show Material materials with Elastic modulus of 60 - 70 GPa at 20.0 °C | 20.0 °C | ||
70 GPa Show Material materials with Elastic modulus of 70 GPa at 23.0 °C | 23.0 °C | ||
69 GPa Show Material materials with Elastic modulus of 69 GPa at 50.0 °C | 50.0 °C | ||
68 GPa Show Material materials with Elastic modulus of 68 GPa at 100.0 °C | 100.0 °C | ||
66 GPa Show Material materials with Elastic modulus of 66 GPa at 150.0 °C | 150.0 °C | ||
63 GPa Show Material materials with Elastic modulus of 63 GPa at 200.0 °C | 200.0 °C | ||
57 GPa Show Material materials with Elastic modulus of 57 GPa at 250.0 °C | 250.0 °C | ||
50 GPa Show Material materials with Elastic modulus of 50 GPa at 300.0 °C | 300.0 °C | ||
Elongation A50 | 3 - 4 % Show Material materials with Elongation A50 of 3 - 4 % at 20.0 °C | 20.0 °C | according to EN 485-2 |
3 - 4 % Show Material materials with Elongation A50 of 3 - 4 % at 23.0 °C | 23.0 °C | according to EN 485-2 | |
Elongation A50, transverse | 3 - 4 % Show Material materials with Elongation A50, transverse of 3 - 4 % at 20.0 °C | 20.0 °C | |
Hardness, Brinell | 35 [-] Show Material materials with Hardness, Brinell of 35 [-] at 20.0 °C | 20.0 °C | |
35 [-] Show Material materials with Hardness, Brinell of 35 [-] at 23.0 °C | 23.0 °C | ||
Hardness, HBW | 26 - 35 [-] Show Material materials with Hardness, HBW of 26 - 35 [-] at 23.0 °C | 23.0 °C | according to EN 485-2 |
Plane-Strain Fracture Toughnes | 22 - 35 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m at 23.0 °C | 23.0 °C | Typical for Wrought 1000 Series Aluminium |
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] at 23.0 °C | 23.0 °C | Typical for Wrought 1000 Series Aluminium |
Shear modulus | 25 GPa Show Material materials with Shear modulus of 25 GPa at 20.0 °C | 20.0 °C | |
26.5 GPa Show Material materials with Shear modulus of 26.5 GPa at 23.0 °C | 23.0 °C | ||
Tensile strength | 110 - 150 MPa Show Material materials with Tensile strength of 110 - 150 MPa at 20.0 °C | 20.0 °C | according to EN 485-2 |
80 - 150 MPa Show Material materials with Tensile strength of 80 - 150 MPa at 23.0 °C | 23.0 °C | according to EN 485-2 | |
Tensile strength, transverse | 110 - 150 MPa Show Material materials with Tensile strength, transverse of 110 - 150 MPa at 20.0 °C | 20.0 °C | |
Yield strength | 50 - 80 MPa Show Material materials with Yield strength of 50 - 80 MPa at 23.0 °C | 23.0 °C | according to EN 485-2 |
Yield strength Rp0.2 | 80 MPa Show Material materials with Yield strength Rp0.2 of 80 MPa at 20.0 °C | 20.0 °C | |
80 MPa Show Material materials with Yield strength Rp0.2 of 80 MPa at 23.0 °C | 23.0 °C | ||
Yield strength Rp0.2, transverse | 80 MPa Show Material materials with Yield strength Rp0.2, transverse of 80 MPa at 20.0 °C | 20.0 °C |
Thermal
Property | Value | Temperature | Comment |
---|---|---|---|
Coefficient of thermal expansion | 2.35E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.35E-5 1/K at 20.0 °C | 20.0 °C | 20-100°C |
2.3E-5 - 2.35E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.3E-5 - 2.35E-5 1/K at 100.0 °C | 100.0 °C | 20-100°C | |
Melting point | 659 °C Show Material materials with Melting point of 659 °C | ||
Specific heat capacity | 921 J/(kg·K) Show Material materials with Specific heat capacity of 921 J/(kg·K) at 20.0 °C | 20.0 °C | |
Thermal conductivity | 215 W/(m·K) Show Material materials with Thermal conductivity of 215 W/(m·K) at 20.0 °C | 20.0 °C | |
138 - 225 W/(m·K) Show Material materials with Thermal conductivity of 138 - 225 W/(m·K) at 23.0 °C | 23.0 °C | ||
Electrical
Property | Value | Temperature |
---|---|---|
Electrical conductivity | 3.64E+7 - 3.70E+7 S/m Show Material materials with Electrical conductivity of 3.64E+7 - 3.70E+7 S/m at 20.0 °C | 20.0 °C |
3.45E+7 - 3.50E+7 S/m Show Material materials with Electrical conductivity of 3.45E+7 - 3.50E+7 S/m at 23.0 °C | 23.0 °C | |
Electrical resistivity | 2.86E-8 - 4.9E-8 Ω·m Show Material materials with Electrical resistivity of 2.86E-8 - 4.9E-8 Ω·m at 23.0 °C | 23.0 °C |
Chemical properties
Property | ||
---|---|---|
Aluminium | 99.8 % | |
Copper | 0.03 % | |
Gallium | 0.03 % | |
Iron | 0.15 % | |
Magnesium | 0.02 % | |
Manganese | 0.02 % | |
Other | 0.02 % | each 0.02,Min. |
Silicon | 0.15 % | |
Titanium | 0.02 % | |
Zinc | 0.06 % |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: very good, Protective: very good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels, Foil for bituminous coating; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Lighting: Anodizing Quality, Lacquering quality; Electronic devices: Housing of devices; Tubes: Industrial tubes, Flexible tube, Pipes; Insulation; Solar: Solar collectors, Photovoltaic panels; Wind energy: Nacelle coverings, Rotor, Hub, Stairs; Cosmetics: Cosmetic pieces; Automotive trim: Interior trim, Windows frame, Marque badges | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Excellent | |
Welding | Excellent | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H14) / very good (H12) |