EN 573-3 Grade AW-5083 H18

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlMg alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.66 g/cm³

Show Material materials with Density of 2.66 g/cm³

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

2.66 g/cm³

Show Material materials with Density of 2.66 g/cm³

H18

EN 573-3

Seamless Tube

20.0 °C

2.64 - 2.66 g/cm³

Show Material materials with Density of 2.64 - 2.66 g/cm³

H18

EN 573-3

Seamless Tube

20.0 °C

2.64 g/cm³

Show Material materials with Density of 2.64 g/cm³

H18

EN 573-3

Seamless Tube

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

71.0 GPa

Show Material materials with Elastic modulus of 71.0 GPa

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

-270.0 °C, 20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H18

EN 573-3

Seamless Tube

20.0 °C

70.0 - 71.0 GPa

Show Material materials with Elastic modulus of 70.0 - 71.0 GPa

H18

EN 573-3

Seamless Tube

20.0 °C

71.0 GPa

Show Material materials with Elastic modulus of 71.0 GPa

H18

EN 573-3

Seamless Tube

50.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H18

EN 573-3

Seamless Tube

100.0 °C

68.0 GPa

Show Material materials with Elastic modulus of 68.0 GPa

H18

EN 573-3

Seamless Tube

150.0 °C

66.0 GPa

Show Material materials with Elastic modulus of 66.0 GPa

H18

EN 573-3

Seamless Tube

200.0 °C

63.0 GPa

Show Material materials with Elastic modulus of 63.0 GPa

H18

EN 573-3

Seamless Tube

250.0 °C

57.0 GPa

Show Material materials with Elastic modulus of 57.0 GPa

H18

EN 573-3

Seamless Tube

300.0 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

H18

EN 573-3

Seamless Tube

Unlock all property charts

Elongation

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

H18

EN 573-3

Seamless Tube

4.0 %

Show Material materials with Elongation of 4.0 %

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A100

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

H18

EN 573-3

Seamless Tube

Shear modulus

26.8 GPa

Show Material materials with Shear modulus of 26.8 GPa

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

26.8 - 27.0 GPa

Show Material materials with Shear modulus of 26.8 - 27.0 GPa

H18

EN 573-3

Seamless Tube

20.0 °C

26.8 GPa

Show Material materials with Shear modulus of 26.8 GPa

H18

EN 573-3

Seamless Tube

Unlock all property charts

Tensile strength

20.0 °C

420.0 MPa

Show Material materials with Tensile strength of 420.0 MPa

H18

EN 573-3

Seamless Tube

-196.0 °C

575.0 MPa

Show Material materials with Tensile strength of 575.0 MPa

H18

EN 573-3

20.0 °C

445.0 MPa

Show Material materials with Tensile strength of 445.0 MPa

H18

EN 573-3

420.0 MPa

Show Material materials with Tensile strength of 420.0 MPa

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Unlock all property charts

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

300 °C, 20 °C, 300.0 °C

2.6e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.6e-05 1/K

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Seamless Tube

200 °C, 20 °C

2.4999999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4999999999999998e-05 1/K

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

100 °C, 20 °C, 100.0 °C

2.42e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.42e-05 1/K

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Seamless Tube

20 °C, -50 °C, -50.0 °C

2.23e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.23e-05 1/K

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Seamless Tube

200.0 °C

2.5e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5e-05 1/K

H18

EN 573-3

Seamless Tube

Unlock all property charts

Max service temperature

-195.0 - 50.0 °C

Show Material materials with Max service temperature of -195.0 - 50.0 °C

H18

EN 573-3

Seamless Tube

Long

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

574.0 - 638.0 °C

Show Material materials with Melting point of 574.0 - 638.0 °C

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Specific heat capacity

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

H18

EN 573-3

Seamless Tube

20.0 °C

899.0 - 900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 899.0 - 900.0 J/(kg·K)

H18

EN 573-3

Seamless Tube

20.0 °C

899.0 J/(kg·K)

Show Material materials with Specific heat capacity of 899.0 J/(kg·K)

H18

EN 573-3

Seamless Tube

Unlock all property charts

Thermal conductivity

20.0 °C

110.0 - 140.0 W/(m·K)

Show Material materials with Thermal conductivity of 110.0 - 140.0 W/(m·K)

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Seamless Tube

20.0 °C

117.0 - 140.0 W/(m·K)

Show Material materials with Thermal conductivity of 117.0 - 140.0 W/(m·K)

H18

EN 573-3

Seamless Tube

20.0 °C

110.0 - 117.0 W/(m·K)

Show Material materials with Thermal conductivity of 110.0 - 117.0 W/(m·K)

H18

EN 573-3

Seamless Tube

20.0 °C

117.0 W/(m·K)

Show Material materials with Thermal conductivity of 117.0 W/(m·K)

H18

EN 573-3

Seamless Tube

Unlock all property charts

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

16000000.0 - 19000000.0 S/m

Show Material materials with Electrical conductivity of 16000000.0 - 19000000.0 S/m

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Seamless Tube

Electrical resistivity

5.26e-08 - 6.25e-08 Ω·m

Show Material materials with Electrical resistivity of 5.26e-08 - 6.25e-08 Ω·m

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

6e-08 Ω·m

Show Material materials with Electrical resistivity of 6e-08 Ω·m

H18

EN 573-3

Seamless Tube

20.0 °C

5.2e-08 - 6e-08 Ω·m

Show Material materials with Electrical resistivity of 5.2e-08 - 6e-08 Ω·m

H18

EN 573-3

Seamless Tube

20.0 °C

6e-08 - 6.2e-08 Ω·m

Show Material materials with Electrical resistivity of 6e-08 - 6.2e-08 Ω·m

H18

EN 573-3

Seamless Tube

20.0 °C

5.2e-08 - 6.2e-08 Ω·m

Show Material materials with Electrical resistivity of 5.2e-08 - 6.2e-08 Ω·m

H18

EN 573-3

Seamless Tube

Unlock all property charts

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.05 - 0.25 %

Show Material materials with Chromium of 0.05 - 0.25 %

H18

EN 573-3, EN 1592

Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Copper

0.1 %

Show Material materials with Copper of 0.1 %

H18

EN 573-3, EN 1592

Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Iron

0.4 %

Show Material materials with Iron of 0.4 %

H18

EN 573-3

Seamless Tube

0.40 %

Show Material materials with Iron of 0.40 %

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Magnesium

4.0 - 4.9 %

Show Material materials with Magnesium of 4.0 - 4.9 %

H18

EN 573-3, EN 1592

Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Manganese

0.4 - 1.0 %

Show Material materials with Manganese of 0.4 - 1.0 %

H18

EN 573-3, EN 1592

Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

H18

EN 573-3, EN 1592

Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

H18

EN 573-3, EN 1592

Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

H18

EN 573-3, EN 1592

Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Technological properties

Property
Anodizing

decorative: sufficient, Protective: good

Brazing

hard brazing (with flux/ without flux): poor / poor, friction soldering: acceptable, soft brazing with flux: poor

Corrosion properties

Seawater: very good, weathering: very good

Workability

Bending / Spinning (cold): good / sufficient, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (O)