General
Property | Value | Temperature |
---|---|---|
Density | 2.64 - 2.66 g/cm³ Show Material materials with Density of 2.64 - 2.66 g/cm³ at 20.0 °C | 20.0 °C |
2.66 g/cm³ Show Material materials with Density of 2.66 g/cm³ at 23.0 °C | 23.0 °C | |
Mechanical
Property | Value | Temperature | Comment |
---|---|---|---|
Elastic modulus | 70 GPa Show Material materials with Elastic modulus of 70 GPa at -270.0 °C | -270.0 °C | |
70 - 71 GPa Show Material materials with Elastic modulus of 70 - 71 GPa at 20.0 °C | 20.0 °C | ||
71 GPa Show Material materials with Elastic modulus of 71 GPa at 23.0 °C | 23.0 °C | ||
69 GPa Show Material materials with Elastic modulus of 69 GPa at 50.0 °C | 50.0 °C | ||
68 GPa Show Material materials with Elastic modulus of 68 GPa at 100.0 °C | 100.0 °C | ||
66 GPa Show Material materials with Elastic modulus of 66 GPa at 150.0 °C | 150.0 °C | ||
63 GPa Show Material materials with Elastic modulus of 63 GPa at 200.0 °C | 200.0 °C | ||
57 GPa Show Material materials with Elastic modulus of 57 GPa at 250.0 °C | 250.0 °C | ||
50 GPa Show Material materials with Elastic modulus of 50 GPa at 300.0 °C | 300.0 °C | ||
Elongation A50 | 2 - 3 % Show Material materials with Elongation A50 of 2 - 3 % at 20.0 °C | 20.0 °C | |
2 - 3 % Show Material materials with Elongation A50 of 2 - 3 % at 23.0 °C | 23.0 °C | ||
Elongation A50, transverse | 2 - 3 % Show Material materials with Elongation A50, transverse of 2 - 3 % at 20.0 °C | 20.0 °C | |
Hardness, Brinell | 106 [-] Show Material materials with Hardness, Brinell of 106 [-] at 20.0 °C | 20.0 °C | |
106 [-] Show Material materials with Hardness, Brinell of 106 [-] at 23.0 °C | 23.0 °C | ||
Plane-Strain Fracture Toughnes | 22 - 35 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] at 20.0 °C | 20.0 °C | |
Shear modulus | 26.8 - 27 GPa Show Material materials with Shear modulus of 26.8 - 27 GPa at 20.0 °C | 20.0 °C | |
26.8 GPa Show Material materials with Shear modulus of 26.8 GPa at 23.0 °C | 23.0 °C | ||
Tensile strength | 360 - 420 MPa Show Material materials with Tensile strength of 360 - 420 MPa at 20.0 °C | 20.0 °C | |
360 - 420 MPa Show Material materials with Tensile strength of 360 - 420 MPa at 23.0 °C | 23.0 °C | ||
Tensile strength, transverse | 360 - 420 MPa Show Material materials with Tensile strength, transverse of 360 - 420 MPa at 20.0 °C | 20.0 °C | |
Yield strength Rp0.2 | 280 MPa Show Material materials with Yield strength Rp0.2 of 280 MPa at 20.0 °C | 20.0 °C | |
280 MPa Show Material materials with Yield strength Rp0.2 of 280 MPa at 23.0 °C | 23.0 °C | ||
Yield strength Rp0.2, transverse | 280 MPa Show Material materials with Yield strength Rp0.2, transverse of 280 MPa at 20.0 °C | 20.0 °C |
Thermal
Property | Value | Temperature | Comment |
---|---|---|---|
Coefficient of thermal expansion | 2.23E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.23E-5 1/K at -50.0 °C | -50.0 °C | |
2.23E-5 - 2.6E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.23E-5 - 2.6E-5 1/K at 20.0 °C | 20.0 °C | ||
2.42E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.42E-5 1/K at 100.0 °C | 100.0 °C | ||
2.5E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.5E-5 1/K at 200.0 °C | 200.0 °C | ||
2.6E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.6E-5 1/K at 300.0 °C | 300.0 °C | ||
Max service temperature | 150 °C Show Material materials with Max service temperature of 150 °C | Typical for Wrought 5000 Series Aluminium | |
Max service temperature, long | -195 - 50 °C Show Material materials with Max service temperature, long of -195 - 50 °C | ||
Melting point | 574 - 638 °C Show Material materials with Melting point of 574 - 638 °C | ||
Specific heat capacity | 899 - 900 J/(kg·K) Show Material materials with Specific heat capacity of 899 - 900 J/(kg·K) at 20.0 °C | 20.0 °C | |
900 J/(kg·K) Show Material materials with Specific heat capacity of 900 J/(kg·K) at 23.0 °C | 23.0 °C | ||
Thermal conductivity | 110 - 140 W/(m·K) Show Material materials with Thermal conductivity of 110 - 140 W/(m·K) at 20.0 °C | 20.0 °C | |
110 - 140 W/(m·K) Show Material materials with Thermal conductivity of 110 - 140 W/(m·K) at 23.0 °C | 23.0 °C | ||
Electrical
Property | Value | Temperature |
---|---|---|
Electrical conductivity | 1.60E+7 - 1.90E+7 S/m Show Material materials with Electrical conductivity of 1.60E+7 - 1.90E+7 S/m at 20.0 °C | 20.0 °C |
1.60E+7 - 1.90E+7 S/m Show Material materials with Electrical conductivity of 1.60E+7 - 1.90E+7 S/m at 23.0 °C | 23.0 °C | |
Electrical resistivity | 5.2E-8 - 6.2E-8 Ω·m Show Material materials with Electrical resistivity of 5.2E-8 - 6.2E-8 Ω·m at 20.0 °C | 20.0 °C |
5.26E-8 - 6.25E-8 Ω·m Show Material materials with Electrical resistivity of 5.26E-8 - 6.25E-8 Ω·m at 23.0 °C | 23.0 °C | |
Chemical properties
Property | ||
---|---|---|
Chromium | 0.05 - 0.25 % | |
Copper | 0.1 % | |
Iron | 0.4 % | |
Magnesium | 4 - 4.9 % | |
Manganese | 0.4 - 1 % | |
Other | each 0.05, total 0.15, Rest Al | |
Silicon | 0.4 % | |
Titanium | 0.15 % | |
Zinc | 0.25 % |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: good | |
Brazing | hard brazing (with flux/ without flux): poor / poor, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good, weathering: very good | |
Workability | Bending / Spinning (cold): good / sufficient, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (O) |