General
Property | Value | Temperature | Comment |
---|---|---|---|
Density | 2.65 - 2.7 g/cm³ Show Material materials with Density of 2.65 - 2.7 g/cm³ at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Mechanical
Property | Value | Temperature | Comment |
---|---|---|---|
Bending Fatigue Strength | 160 MPa Show Material materials with Bending Fatigue Strength of 160 MPa at 23.0 °C | 23.0 °C | |
Elastic modulus | 69 - 70 GPa Show Material materials with Elastic modulus of 69 - 70 GPa at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Elongation A100 | 10 - 14 % Show Material materials with Elongation A100 of 10 - 14 % at 23.0 °C | 23.0 °C | |
Elongation A50 | 10 - 12 % Show Material materials with Elongation A50 of 10 - 12 % at 23.0 °C | 23.0 °C | |
Plane-Strain Fracture Toughnes | 22 - 35 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Shear modulus | 26 - 26.5 GPa Show Material materials with Shear modulus of 26 - 26.5 GPa at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Tensile strength | 285 - 385 MPa Show Material materials with Tensile strength of 285 - 385 MPa at 23.0 °C | 23.0 °C | |
Yield strength Rp0.2 | 200 - 295 MPa Show Material materials with Yield strength Rp0.2 of 200 - 295 MPa at 23.0 °C | 23.0 °C |
Thermal
Property | Value | Temperature | Comment |
---|---|---|---|
Coefficient of thermal expansion | 2.2E-5 - 2.5E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.2E-5 - 2.5E-5 1/K at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Max service temperature | 150 °C Show Material materials with Max service temperature of 150 °C | Typical for Wrought 5000 Series Aluminium | |
Melting point | 560 - 655 °C Show Material materials with Melting point of 560 - 655 °C | Typical for Wrought 5000 Series Aluminium | |
Specific heat capacity | 879 - 963 J/(kg·K) Show Material materials with Specific heat capacity of 879 - 963 J/(kg·K) at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Thermal conductivity | 112 - 205 W/(m·K) Show Material materials with Thermal conductivity of 112 - 205 W/(m·K) at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Electrical
Property | Value | Temperature | Comment |
---|---|---|---|
Electrical conductivity | 1.80E+7 - 3.10E+7 S/m Show Material materials with Electrical conductivity of 1.80E+7 - 3.10E+7 S/m at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Electrical resistivity | 3.3E-8 - 5E-8 Ω·m Show Material materials with Electrical resistivity of 3.3E-8 - 5E-8 Ω·m at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Chemical properties
Property | ||
---|---|---|
Chromium | 0.05 - 0.25 % | |
Copper | 0.1 % | |
Iron | 0.4 % | |
Magnesium | 4 - 4.9 % | |
Manganese | 0.4 - 1 % | |
Other | each 0.05, total 0.15, Rest Al | |
Silicon | 0.4 % | |
Titanium | 0.15 % | |
Zinc | 0.25 % |
Technological properties
Property | ||
---|---|---|
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: kein Schadensfall im Betrieb und bei Labortests (O, H321, H116), kein Schadensfall im Betrieb, eingeschränkte Schäden bei den Labortests (H111), general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: poor | |
Workability | general (condition): acceptable (O), poor(H321, H116, H111) |