EN 573-3 Grade AW-5086 F

Want to keep this datasheet? Save it now in your required format

Description

Aluminum EN AW-5086 is structural alloy, which offers users strong corrosion resistance and high electrical conductivity. Offering higher strength levels than 5052 or 5083, EN AW-5086 becomes stronger with stain hardening and cold working, all while remaining a cost-effective choice. It can be welded with conventional methods, though electric arc welding is preferred.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.66 g/cm³

Show Material materials with Density of 2.66 g/cm³

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20.0 °C

2.66 g/cm³

Show Material materials with Density of 2.66 g/cm³

F

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

2.66 - 2.67 g/cm³

Show Material materials with Density of 2.66 - 2.67 g/cm³

F

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

2.67 g/cm³

Show Material materials with Density of 2.67 g/cm³

F

EN 573-3

Profile, Rod, Flat, Tube

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

71.0 GPa

Show Material materials with Elastic modulus of 71.0 GPa

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20.0 °C

71.0 GPa

Show Material materials with Elastic modulus of 71.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube

Elongation

10.0 %

Show Material materials with Elongation of 10.0 %

F

EN 573-3, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

A50

12.0 %

Show Material materials with Elongation of 12.0 %

F

EN 573-3, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

A100

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

F

EN 573-3

Profile, Rod, Tube

A50

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

F

EN 573-3

Profile, Rod, Tube

Hardness, Brinell

20.0 °C

65.0 [-]

Show Material materials with Hardness, Brinell of 65.0 [-]

F

EN 573-3

Profile, Rod, Tube

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

F

EN 573-3

Profile, Rod, Flat, Tube

Shear modulus

26.7 GPa

Show Material materials with Shear modulus of 26.7 GPa

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20.0 °C

26.7 - 27.0 GPa

Show Material materials with Shear modulus of 26.7 - 27.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

26.7 GPa

Show Material materials with Shear modulus of 26.7 GPa

F

EN 573-3

Profile, Rod, Flat, Tube

Tensile strength

240.0 MPa

Show Material materials with Tensile strength of 240.0 MPa

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20.0 °C

240.0 MPa

Show Material materials with Tensile strength of 240.0 MPa

F

EN 573-3

Profile, Rod, Tube, Flat

20.0 °C

240.0 MPa

Show Material materials with Tensile strength of 240.0 MPa

F

EN 573-3

Flat

Transverse

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

-50 °C

2.2e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2e-05 1/K

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Profile, Flat

-50.0 °C

2.2e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2e-05 1/K

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Profile, Flat

20 °C

2.2e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2e-05 1/K

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Profile, Flat

20 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Profile, Flat

20 °C

2.4699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4699999999999997e-05 1/K

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20 °C

2.58e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.58e-05 1/K

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Profile, Flat

100 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Profile, Flat

100.0 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Profile, Flat

200 °C

2.4699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4699999999999997e-05 1/K

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

200.0 °C

2.47e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.47e-05 1/K

F

EN 573-3

Profile, Rod, Flat, Tube

300 °C

2.58e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.58e-05 1/K

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Profile, Flat

300.0 °C

2.58e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.58e-05 1/K

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Profile, Flat

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

585.0 - 641.0 °C

Show Material materials with Melting point of 585.0 - 641.0 °C

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

585.0 - 640.0 °C

Show Material materials with Melting point of 585.0 - 640.0 °C

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Specific heat capacity

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20.0 °C

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

F

EN 573-3

Profile, Rod, Flat, Tube

Thermal conductivity

126 W/(m·K)

Show Material materials with Thermal conductivity of 126 W/(m·K)

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20.0 °C

120.0 - 140.0 W/(m·K)

Show Material materials with Thermal conductivity of 120.0 - 140.0 W/(m·K)

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Profile, Flat

20.0 °C

120.0 - 126.0 W/(m·K)

Show Material materials with Thermal conductivity of 120.0 - 126.0 W/(m·K)

F

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

126.0 - 140.0 W/(m·K)

Show Material materials with Thermal conductivity of 126.0 - 140.0 W/(m·K)

F

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

126.0 W/(m·K)

Show Material materials with Thermal conductivity of 126.0 W/(m·K)

F

EN 573-3

Profile, Rod, Flat, Tube

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

18000000.0 S/m

Show Material materials with Electrical conductivity of 18000000.0 S/m

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20.0 °C

17000000.0 - 19000000.0 S/m

Show Material materials with Electrical conductivity of 17000000.0 - 19000000.0 S/m

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Profile, Flat

Electrical resistivity

5.26e-08 - 5.88e-08 Ω·m

Show Material materials with Electrical resistivity of 5.26e-08 - 5.88e-08 Ω·m

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

5.56e-08 Ω·m

Show Material materials with Electrical resistivity of 5.56e-08 Ω·m

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20.0 °C

5.2e-08 - 5.6e-08 Ω·m

Show Material materials with Electrical resistivity of 5.2e-08 - 5.6e-08 Ω·m

F

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

5.2e-08 - 5.8e-08 Ω·m

Show Material materials with Electrical resistivity of 5.2e-08 - 5.8e-08 Ω·m

F

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

5.6e-08 Ω·m

Show Material materials with Electrical resistivity of 5.6e-08 Ω·m

F

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

5.6e-08 - 5.8e-08 Ω·m

Show Material materials with Electrical resistivity of 5.6e-08 - 5.8e-08 Ω·m

F

EN 573-3

Profile, Rod, Flat, Tube

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.05 - 0.25 %

Show Material materials with Chromium of 0.05 - 0.25 %

F

EN 573-3, EN 485, EN 755

Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Welded Tube, Wire

Copper

0.1 %

Show Material materials with Copper of 0.1 %

F

EN 573-3, EN 485, EN 755

Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Welded Tube, Wire

Iron

0.5 %

Show Material materials with Iron of 0.5 %

F

EN 573-3

Profile, Rod, Flat, Tube

0.50 %

Show Material materials with Iron of 0.50 %

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Magnesium

3.5 - 4.5 %

Show Material materials with Magnesium of 3.5 - 4.5 %

F

EN 573-3, EN 485, EN 755

Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Welded Tube, Wire

Manganese

0.2 - 0.7 %

Show Material materials with Manganese of 0.2 - 0.7 %

F

EN 573-3, EN 485, EN 755

Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Welded Tube, Wire

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

F

EN 573-3, EN 485, EN 755

Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Welded Tube, Wire

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

F

EN 573-3, EN 485, EN 755

Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Welded Tube, Wire

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

F

EN 573-3, EN 485, EN 755

Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Welded Tube, Wire

Technological properties

Property
Anodizing

decorative: acceptable, Protective: very good

Brazing

hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor

Workability

Bending / Spinning (cold): good / sufficient, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (O)