General
Property | Value | Temperature |
---|---|---|
Density | 2.66 - 2.67 g/cm³ Show Material materials with Density of 2.66 - 2.67 g/cm³ at 20.0 °C | 20.0 °C |
2.66 g/cm³ Show Material materials with Density of 2.66 g/cm³ at 23.0 °C | 23.0 °C | |
Dimension
Property | Value |
---|---|
Thickness | 0.2 - 4 mm Show Material materials with Thickness of 0.2 - 4 mm |
Mechanical
Property | Value | Temperature | Comment |
---|---|---|---|
Elastic modulus | 71 GPa Show Material materials with Elastic modulus of 71 GPa at 20.0 °C | 20.0 °C | |
71 GPa Show Material materials with Elastic modulus of 71 GPa at 23.0 °C | 23.0 °C | ||
Elongation | 2 - 5 % Show Material materials with Elongation of 2 - 5 % at 20.0 °C | 20.0 °C | |
Elongation A100 | 2 - 5 % Show Material materials with Elongation A100 of 2 - 5 % at 23.0 °C | 23.0 °C | |
Elongation A50 | 1 - 2 % Show Material materials with Elongation A50 of 1 - 2 % at 20.0 °C | 20.0 °C | |
1 - 2 % Show Material materials with Elongation A50 of 1 - 2 % at 23.0 °C | 23.0 °C | ||
Elongation A50, transverse | 1 - 2 % Show Material materials with Elongation A50, transverse of 1 - 2 % at 20.0 °C | 20.0 °C | |
Hardness, Brinell | 98 - 100 [-] Show Material materials with Hardness, Brinell of 98 - 100 [-] at 20.0 °C | 20.0 °C | |
98 [-] Show Material materials with Hardness, Brinell of 98 [-] at 23.0 °C | 23.0 °C | ||
Hardness, HBW | 98 [-] Show Material materials with Hardness, HBW of 98 [-] at 23.0 °C | 23.0 °C | |
Plane-Strain Fracture Toughnes | 22 - 35 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] at 20.0 °C | 20.0 °C | |
Shear modulus | 26.7 - 27 GPa Show Material materials with Shear modulus of 26.7 - 27 GPa at 20.0 °C | 20.0 °C | |
26.7 - 27 GPa Show Material materials with Shear modulus of 26.7 - 27 GPa at 23.0 °C | 23.0 °C | ||
Tensile strength | 320 - 385 MPa Show Material materials with Tensile strength of 320 - 385 MPa at 20.0 °C | 20.0 °C | |
320 - 385 MPa Show Material materials with Tensile strength of 320 - 385 MPa at 23.0 °C | 23.0 °C | ||
Tensile strength, transverse | 325 - 385 MPa Show Material materials with Tensile strength, transverse of 325 - 385 MPa at 20.0 °C | 20.0 °C | |
Yield strength | 270 MPa Show Material materials with Yield strength of 270 MPa at 23.0 °C | 23.0 °C | |
Yield strength Rp0.2 | 260 - 270 MPa Show Material materials with Yield strength Rp0.2 of 260 - 270 MPa at 20.0 °C | 20.0 °C | |
260 - 270 MPa Show Material materials with Yield strength Rp0.2 of 260 - 270 MPa at 23.0 °C | 23.0 °C | ||
Yield strength Rp0.2, transverse | 270 MPa Show Material materials with Yield strength Rp0.2, transverse of 270 MPa at 20.0 °C | 20.0 °C |
Thermal
Property | Value | Temperature | Comment |
---|---|---|---|
Coefficient of thermal expansion | 2.2E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.2E-5 1/K at -50.0 °C | -50.0 °C | 20-100°C |
2.2E-5 - 2.58E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.2E-5 - 2.58E-5 1/K at 20.0 °C | 20.0 °C | 20-100°C | |
2.38E-5 - 2.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.38E-5 - 2.4E-5 1/K at 100.0 °C | 100.0 °C | 20-100°C | |
2.47E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.47E-5 1/K at 200.0 °C | 200.0 °C | 20-100°C | |
2.58E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.58E-5 1/K at 300.0 °C | 300.0 °C | 20-100°C | |
Max service temperature | 150 °C Show Material materials with Max service temperature of 150 °C | Typical for Wrought 5000 Series Aluminium | |
Melting point | 585 - 641 °C Show Material materials with Melting point of 585 - 641 °C | ||
Specific heat capacity | 900 J/(kg·K) Show Material materials with Specific heat capacity of 900 J/(kg·K) at 20.0 °C | 20.0 °C | |
900 J/(kg·K) Show Material materials with Specific heat capacity of 900 J/(kg·K) at 23.0 °C | 23.0 °C | ||
Thermal conductivity | 120 - 140 W/(m·K) Show Material materials with Thermal conductivity of 120 - 140 W/(m·K) at 20.0 °C | 20.0 °C | |
120 - 140 W/(m·K) Show Material materials with Thermal conductivity of 120 - 140 W/(m·K) at 23.0 °C | 23.0 °C | ||
Electrical
Property | Value | Temperature |
---|---|---|
Electrical conductivity | 1.70E+7 - 1.90E+7 S/m Show Material materials with Electrical conductivity of 1.70E+7 - 1.90E+7 S/m at 20.0 °C | 20.0 °C |
1.70E+7 - 1.90E+7 S/m Show Material materials with Electrical conductivity of 1.70E+7 - 1.90E+7 S/m at 23.0 °C | 23.0 °C | |
Electrical resistivity | 5.2E-8 - 5.8E-8 Ω·m Show Material materials with Electrical resistivity of 5.2E-8 - 5.8E-8 Ω·m at 20.0 °C | 20.0 °C |
5.26E-8 - 5.88E-8 Ω·m Show Material materials with Electrical resistivity of 5.26E-8 - 5.88E-8 Ω·m at 23.0 °C | 23.0 °C | |
Chemical properties
Property | ||
---|---|---|
Chromium | 0.05 - 0.25 % | |
Copper | 0.1 % | |
Iron | 0.5 % | |
Magnesium | 3.5 - 4.5 % | |
Manganese | 0.2 - 0.7 % | |
Other | 0.05 - 0.15 % | each 0.05, total 0.15, Rest Al |
Silicon | 0.4 % | |
Titanium | 0.15 % | |
Zinc | 0.25 % |
Technological properties
Property | ||
---|---|---|
Anodizing | Excellent (anodizing quality) | |
Application areas | Vessels: Pressure, Cryogenics; Components: Access hatches, Spoilers, General tranportation | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Excellent | |
Welding | Good | |
Workability | Good (in O temper) |