EN 573-3 Grade AW-5086 H244

Want to keep this datasheet? Save it now in your required format

Description

Aluminum EN AW-5086 is structural alloy, which offers users strong corrosion resistance and high electrical conductivity. Offering higher strength levels than 5052 or 5083, EN AW-5086 becomes stronger with stain hardening and cold working, all while remaining a cost-effective choice. It can be welded with conventional methods, though electric arc welding is preferred.

Related Standards

Equivalent Materials

This material data has been provided by AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated StandardsShape

Density

2.66 g/cm³

Show Material materials with Density of 2.66 g/cm³

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Mechanical

PropertyValueConditionRelated StandardsShapeComment

Bending angle 90°

4.0 °/t

Show Material materials with Bending angle 90° of 4.0 °/t

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

4.5 °/t

Show Material materials with Bending angle 90° of 4.5 °/t

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

5.5 °/t

Show Material materials with Bending angle 90° of 5.5 °/t

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Elastic modulus

71.0 GPa

Show Material materials with Elastic modulus of 71.0 GPa

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 5000 Series Aluminium

Shear modulus

26.7 GPa

Show Material materials with Shear modulus of 26.7 GPa

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Tensile strength

300.0 - 360.0 MPa

Show Material materials with Tensile strength of 300.0 - 360.0 MPa

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

-50 °C

2.2e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2e-05 1/K

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20 °C

2.2e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2e-05 1/K

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20 °C

2.4699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4699999999999997e-05 1/K

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20 °C

2.58e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.58e-05 1/K

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

100 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

200 °C

2.4699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4699999999999997e-05 1/K

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

300 °C

2.58e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.58e-05 1/K

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

585.0 - 641.0 °C

Show Material materials with Melting point of 585.0 - 641.0 °C

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

585.0 - 640.0 °C

Show Material materials with Melting point of 585.0 - 640.0 °C

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Specific heat capacity

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Thermal conductivity

120.0 - 140.0 W/(m·K)

Show Material materials with Thermal conductivity of 120.0 - 140.0 W/(m·K)

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

126 W/(m·K)

Show Material materials with Thermal conductivity of 126 W/(m·K)

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Electrical

PropertyValueConditionRelated StandardsShape

Electrical conductivity

17000000.0 - 19000000.0 S/m

Show Material materials with Electrical conductivity of 17000000.0 - 19000000.0 S/m

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

18000000.0 S/m

Show Material materials with Electrical conductivity of 18000000.0 S/m

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Electrical resistivity

5.26e-08 - 5.88e-08 Ω·m

Show Material materials with Electrical resistivity of 5.26e-08 - 5.88e-08 Ω·m

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

5.56e-08 Ω·m

Show Material materials with Electrical resistivity of 5.56e-08 Ω·m

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.05 - 0.25 %

Show Material materials with Chromium of 0.05 - 0.25 %

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Copper

0.1 %

Show Material materials with Copper of 0.1 %

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Iron

0.50 %

Show Material materials with Iron of 0.50 %

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Magnesium

3.5 - 4.5 %

Show Material materials with Magnesium of 3.5 - 4.5 %

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Manganese

0.2 - 0.7 %

Show Material materials with Manganese of 0.2 - 0.7 %

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

H244

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Technological properties

Property
Anodizing

decorative: acceptable, Protective: very good

Brazing

hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor

Workability

Bending / Spinning (cold): good / sufficient, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (O)