General
Property | Value | Temperature |
---|---|---|
Density | 2.64 g/cm³ Show Material materials with Density of 2.64 g/cm³ at 20.0 °C | 20.0 °C |
2.65 g/cm³ Show Material materials with Density of 2.65 g/cm³ at 23.0 °C | 23.0 °C | |
Dimension
Property | Value |
---|---|
Thickness | 0.2 - 3 mm Show Material materials with Thickness of 0.2 - 3 mm |
Mechanical
Property | Value | Temperature | Comment |
---|---|---|---|
Bending angle 180° | 1 - 2 °/t Show Material materials with Bending angle 180° of 1 - 2 °/t at 23.0 °C | 23.0 °C | |
Elastic modulus | 70 - 71 GPa Show Material materials with Elastic modulus of 70 - 71 GPa at 23.0 °C | 23.0 °C | |
Elongation A100 | 26 % Show Material materials with Elongation A100 of 26 % at 23.0 °C | 23.0 °C | |
Elongation A50 | 11 - 13 % Show Material materials with Elongation A50 of 11 - 13 % at 20.0 °C | 20.0 °C | |
11 - 13 % Show Material materials with Elongation A50 of 11 - 13 % at 23.0 °C | 23.0 °C | ||
Elongation A50, transverse | 11 - 13 % Show Material materials with Elongation A50, transverse of 11 - 13 % at 20.0 °C | 20.0 °C | |
Hardness, Brinell | 69 [-] Show Material materials with Hardness, Brinell of 69 [-] at 20.0 °C | 20.0 °C | |
69 [-] Show Material materials with Hardness, Brinell of 69 [-] at 23.0 °C | 23.0 °C | ||
Hardness, HBW | 69 [-] Show Material materials with Hardness, HBW of 69 [-] at 23.0 °C | 23.0 °C | |
Plane-Strain Fracture Toughnes | 22 - 35 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Shear modulus | 27 GPa Show Material materials with Shear modulus of 27 GPa at 20.0 °C | 20.0 °C | |
27 GPa Show Material materials with Shear modulus of 27 GPa at 23.0 °C | 23.0 °C | ||
Tensile strength | 255 - 315 MPa Show Material materials with Tensile strength of 255 - 315 MPa at 20.0 °C | 20.0 °C | |
255 - 350 MPa Show Material materials with Tensile strength of 255 - 350 MPa at 23.0 °C | 23.0 °C | ||
Tensile strength, transverse | 255 - 315 MPa Show Material materials with Tensile strength, transverse of 255 - 315 MPa at 20.0 °C | 20.0 °C | |
Yield strength | 110 MPa Show Material materials with Yield strength of 110 MPa at 23.0 °C | 23.0 °C | |
Yield strength Rp0.2 | 110 MPa Show Material materials with Yield strength Rp0.2 of 110 MPa at 20.0 °C | 20.0 °C | |
110 - 125 MPa Show Material materials with Yield strength Rp0.2 of 110 - 125 MPa at 23.0 °C | 23.0 °C | ||
Yield strength Rp0.2, transverse | 110 MPa Show Material materials with Yield strength Rp0.2, transverse of 110 MPa at 20.0 °C | 20.0 °C |
Thermal
Property | Value | Temperature | Comment |
---|---|---|---|
Coefficient of thermal expansion | 2.32E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.32E-5 1/K at 20.0 °C | 20.0 °C | 20-100°C |
2.32E-5 - 2.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.32E-5 - 2.4E-5 1/K at 100.0 °C | 100.0 °C | 20-100°C | |
Max service temperature | 150 °C Show Material materials with Max service temperature of 150 °C | Typical for Wrought 5000 Series Aluminium | |
Melting point | 577 - 638 °C Show Material materials with Melting point of 577 - 638 °C | ||
Specific heat capacity | 900 J/(kg·K) Show Material materials with Specific heat capacity of 900 J/(kg·K) at 20.0 °C | 20.0 °C | |
Thermal conductivity | 140 W/(m·K) Show Material materials with Thermal conductivity of 140 W/(m·K) at 20.0 °C | 20.0 °C | |
121 - 123 W/(m·K) Show Material materials with Thermal conductivity of 121 - 123 W/(m·K) at 23.0 °C | 23.0 °C | ||
Electrical
Property | Value | Temperature |
---|---|---|
Electrical conductivity | 1.90E+7 S/m Show Material materials with Electrical conductivity of 1.90E+7 S/m at 20.0 °C | 20.0 °C |
1.80E+7 S/m Show Material materials with Electrical conductivity of 1.80E+7 S/m at 23.0 °C | 23.0 °C | |
Electrical resistivity | 5.56E-8 - 5.6E-8 Ω·m Show Material materials with Electrical resistivity of 5.56E-8 - 5.6E-8 Ω·m at 23.0 °C | 23.0 °C |
Chemical properties
Property | ||
---|---|---|
Chromium | 0.1 % | |
Copper | 0.15 % | |
Iron | 0.35 % | |
Magnesium | 4 - 5 % | |
Manganese | 0.2 - 0.5 % | |
Other | 0.05 - 0.15 % | each 0.05, total 0.15, Rest Al |
Silicon | 0.2 % | |
Titanium | 0.1 % | |
Zinc | 0.25 % |
Technological properties
Property | ||
---|---|---|
Anodizing | Excellent | |
Application areas | Wind energy: Nacelle coverings, rotor hub, stairs; Components: Heat shields, Access hatches, Spoilers, General tranportation | |
Brazing | Brazing is not recommended. | |
Corrosion properties | Excellent | |
Welding | Good | |
Workability | Very good in special (Lüder lines resistant) O temper. |