EN 573-3 Grade AW-5251 H14

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlMg alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey,Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.68 g/cm³

Show Material materials with Density of 2.68 g/cm³

H14

EN 573-3, EN 1301, EN 1592, EN 485, EN 754

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

20.0 °C

2.68 g/cm³

Show Material materials with Density of 2.68 g/cm³

H14

EN 573-3

Rod, Flat, Seamless Tube, Tube, Wire

20.0 °C

2.68 - 2.69 g/cm³

Show Material materials with Density of 2.68 - 2.69 g/cm³

H14

EN 573-3

Rod, Flat, Seamless Tube, Tube, Wire

20.0 °C

2.69 g/cm³

Show Material materials with Density of 2.69 g/cm³

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3

Coil, Sheet, Plate, Strip, Rod, Flat, Seamless Tube, Tube, Wire

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.2 mm

Show Material materials with Thickness of 0.2 mm

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2

0.2 mm

Coil, Sheet, Plate, Strip

6.0 mm

Show Material materials with Thickness of 6.0 mm

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2

6.0 mm

Coil, Sheet, Plate, Strip

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

115.0 MPa

Show Material materials with Bending Fatigue Strength of 115.0 MPa

H14

EN 573-3, EN 1301, EN 1592, EN 485, EN 754

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

Bending angle 180°

2.5 °/t

Show Material materials with Bending angle 180° of 2.5 °/t

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

2.5 °/t

Show Material materials with Bending angle 180° of 2.5 °/t

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

Bending angle 90°

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

1.5 °/t

Show Material materials with Bending angle 90° of 1.5 °/t

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

2.5 °/t

Show Material materials with Bending angle 90° of 2.5 °/t

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

2.5 °/t

Show Material materials with Bending angle 90° of 2.5 °/t

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

3.0 °/t

Show Material materials with Bending angle 90° of 3.0 °/t

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

Elastic modulus

68.6 GPa

Show Material materials with Elastic modulus of 68.6 GPa

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H14

EN 573-3, EN 1301, EN 1592, EN 485, EN 754

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H14

EN 573-3

Rod, Flat, Seamless Tube, Tube, Wire

Elongation

2.0 %

Show Material materials with Elongation of 2.0 %

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

A50

2.0 - 4.0 %

Show Material materials with Elongation of 2.0 - 4.0 %

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

A50

3.0 %

Show Material materials with Elongation of 3.0 %

H14

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

A50

4.0 %

Show Material materials with Elongation of 4.0 %

H14

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

A50

4.0 %

Show Material materials with Elongation of 4.0 %

H14

EN 573-3, EN 1301

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

4.0 %

Show Material materials with Elongation of 4.0 %

H14

EN 573-3, EN 754

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

A100

5.0 %

Show Material materials with Elongation of 5.0 %

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

A50

5.0 %

Show Material materials with Elongation of 5.0 %

H14

EN 573-3, EN 754

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

A100

6.0 %

Show Material materials with Elongation of 6.0 %

H14

EN 573-3, EN 1592

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

A100

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H14

EN 573-3

Flat

A50

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H14

EN 573-3

Flat

A50 Transverse

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

H14

EN 573-3

Tube, Flat

A50

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

H14

EN 573-3

Flat

A50 Transverse

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

H14

EN 573-3

Rod, Flat

A50

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

H14

EN 573-3

Tube

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

H14

EN 573-3

Flat

A50 Transverse

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H14

EN 573-3

Flat

A50

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H14

EN 573-3

Rod

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H14

EN 573-3

Flat

A50 Transverse

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

H14

EN 573-3

Seamless Tube

Unlock all property charts

Hardness, Brinell

64.0 [-]

Show Material materials with Hardness, Brinell of 64.0 [-]

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

20.0 °C

64.0 [-]

Show Material materials with Hardness, Brinell of 64.0 [-]

H14

EN 573-3

Flat

20.0 °C

65.0 [-]

Show Material materials with Hardness, Brinell of 65.0 [-]

H14

EN 573-3

Rod, Tube

Unlock all property charts

Hardness, HBW

64 [-]

Show Material materials with Hardness, HBW of 64 [-]

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

H14

EN 573-3

Rod, Flat, Seamless Tube, Tube, Wire

Shear modulus

26.3 GPa

Show Material materials with Shear modulus of 26.3 GPa

H14

EN 573-3, EN 1301, EN 1592, EN 485, EN 754

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

20.0 °C

26.3 - 26.5 GPa

Show Material materials with Shear modulus of 26.3 - 26.5 GPa

H14

EN 573-3

Rod, Flat, Seamless Tube, Tube, Wire

20.0 °C

26.3 GPa

Show Material materials with Shear modulus of 26.3 GPa

H14

EN 573-3

Rod, Flat, Seamless Tube, Tube, Wire

Unlock all property charts

Tensile strength

215.0 - 265.0 MPa

Show Material materials with Tensile strength of 215.0 - 265.0 MPa

H14

EN 573-3, EN 1301

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

230.0 MPa

Show Material materials with Tensile strength of 230.0 MPa

H14

EN 573-3, EN 1592

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

20.0 °C

200.0 - 240.0 MPa

Show Material materials with Tensile strength of 200.0 - 240.0 MPa

H14

EN 573-3, EN 754

Rod, Tube, Strip, Sheet, Plate, Wire, Welded Tube, Bar

20.0 °C

210.0 - 250.0 MPa

Show Material materials with Tensile strength of 210.0 - 250.0 MPa

H14

EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Flat, Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar, Coil, Sheet, Plate, Strip

20.0 °C

210.0 - 250.0 MPa

Show Material materials with Tensile strength of 210.0 - 250.0 MPa

H14

EN 573-3

Flat

Transverse

20.0 °C

230.0 MPa

Show Material materials with Tensile strength of 230.0 MPa

H14

EN 573-3

Seamless Tube

Unlock all property charts

Yield strength

160.0 MPa

Show Material materials with Yield strength of 160.0 MPa

H14

EN 573-3, EN 754

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

RP02

170.0 MPa

Show Material materials with Yield strength of 170.0 MPa

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

RP02

170 MPa

Show Material materials with Yield strength of 170 MPa

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

190.0 MPa

Show Material materials with Yield strength of 190.0 MPa

H14

EN 573-3, EN 1592

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

RP02

220.0 MPa

Show Material materials with Yield strength of 220.0 MPa

H14

EN 573-3, EN 1301

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

RP02

20.0 °C

160.0 MPa

Show Material materials with Yield strength of 160.0 MPa

H14

EN 573-3

Rod, Tube

RP02

20.0 °C

170.0 MPa

Show Material materials with Yield strength of 170.0 MPa

H14

EN 573-3

Flat

RP02

20.0 °C

170.0 MPa

Show Material materials with Yield strength of 170.0 MPa

H14

EN 573-3

Flat

RP02 Transverse

20.0 °C

190.0 MPa

Show Material materials with Yield strength of 190.0 MPa

H14

EN 573-3

Seamless Tube

RP02

Unlock all property charts

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.3699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3699999999999997e-05 1/K

H14

EN 573-3, EN 1301, EN 1592, EN 485, EN 754

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

100 °C

2.3699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3699999999999997e-05 1/K

H14

EN 573-3, EN 1301, EN 1592, EN 485, EN 754

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

20-100°C

Unlock all property charts

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

610.0 - 650.0 °C

Show Material materials with Melting point of 610.0 - 650.0 °C

H14

EN 573-3, EN 1301, EN 1592, EN 485, EN 754

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

Specific heat capacity

20.0 °C

898.0 - 921.0 J/(kg·K)

Show Material materials with Specific heat capacity of 898.0 - 921.0 J/(kg·K)

H14

EN 573-3

Rod, Flat, Seamless Tube, Tube, Wire

20.0 °C

898.0 J/(kg·K)

Show Material materials with Specific heat capacity of 898.0 J/(kg·K)

H14

EN 573-3

Rod, Flat, Seamless Tube, Tube, Wire

20.0 °C

921.0 J/(kg·K)

Show Material materials with Specific heat capacity of 921.0 J/(kg·K)

H14

EN 573-3

Rod, Flat, Seamless Tube, Tube, Wire

Unlock all property charts

Thermal conductivity

140.0 - 160.0 W/(m·K)

Show Material materials with Thermal conductivity of 140.0 - 160.0 W/(m·K)

H14

EN 573-3, EN 1301, EN 1592, EN 485, EN 754

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

153 W/(m·K)

Show Material materials with Thermal conductivity of 153 W/(m·K)

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

20.0 °C

149.0 - 167.0 W/(m·K)

Show Material materials with Thermal conductivity of 149.0 - 167.0 W/(m·K)

H14

EN 573-3

Rod, Flat, Seamless Tube, Tube, Wire

20.0 °C

149.0 W/(m·K)

Show Material materials with Thermal conductivity of 149.0 W/(m·K)

H14

EN 573-3

Rod, Flat, Seamless Tube, Tube, Wire

Unlock all property charts

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

25000000.0 - 30000000.0 S/m

Show Material materials with Electrical conductivity of 25000000.0 - 30000000.0 S/m

H14

EN 573-3, EN 1301, EN 1592, EN 485, EN 754

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

20.0 °C

26000000.0 S/m

Show Material materials with Electrical conductivity of 26000000.0 S/m

H14

EN 573-3

Rod, Flat, Seamless Tube, Tube, Wire

Electrical resistivity

3.33e-08 - 4e-08 Ω·m

Show Material materials with Electrical resistivity of 3.33e-08 - 4e-08 Ω·m

H14

EN 573-3, EN 1301, EN 1592, EN 485, EN 754

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

4.5e-08 Ω·m

Show Material materials with Electrical resistivity of 4.5e-08 Ω·m

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

20.0 °C

4.6e-08 Ω·m

Show Material materials with Electrical resistivity of 4.6e-08 Ω·m

H14

EN 573-3

Rod, Flat, Seamless Tube, Tube, Wire

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.15 %

Show Material materials with Chromium of 0.15 %

H14

EN 573-3, EN 1301, EN 1592, EN 485, EN 754

Rod, Flat, Seamless Tube, Tube, Wire, Strip, Sheet, Plate, Welded Tube, Bar

0.15 %

Show Material materials with Chromium of 0.15 %

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

Copper

0.15 %

Show Material materials with Copper of 0.15 %

H14

EN 573-3, EN 1301, EN 1592, EN 485, EN 754

Rod, Flat, Seamless Tube, Tube, Wire, Strip, Sheet, Plate, Welded Tube, Bar

0.15 %

Show Material materials with Copper of 0.15 %

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

Iron

0.5 %

Show Material materials with Iron of 0.5 %

H14

EN 573-3

Rod, Flat, Seamless Tube, Tube, Wire

0.50 %

Show Material materials with Iron of 0.50 %

H14

EN 573-3, EN 1301, EN 1592, EN 485, EN 754

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

0.5 %

Show Material materials with Iron of 0.5 %

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

Magnesium

1.7 - 2.4 %

Show Material materials with Magnesium of 1.7 - 2.4 %

H14

EN 573-3, EN 1301, EN 1592, EN 485, EN 754, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Rod, Flat, Seamless Tube, Tube, Wire, Strip, Sheet, Plate, Welded Tube, Bar, Coil, Sheet, Plate, Strip

Manganese

0.1 - 0.5 %

Show Material materials with Manganese of 0.1 - 0.5 %

H14

EN 573-3, EN 1301, EN 1592, EN 485, EN 754, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Rod, Flat, Seamless Tube, Tube, Wire, Strip, Sheet, Plate, Welded Tube, Bar, Coil, Sheet, Plate, Strip

Other

0.05 - 0.15 %

Show Material materials with Other of 0.05 - 0.15 %

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

H14

EN 573-3, EN 1301, EN 1592, EN 485, EN 754

Rod, Flat, Seamless Tube, Tube, Wire, Strip, Sheet, Plate, Welded Tube, Bar

0.4 %

Show Material materials with Silicon of 0.4 %

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

H14

EN 573-3, EN 1301, EN 1592, EN 485, EN 754

Rod, Flat, Seamless Tube, Tube, Wire, Strip, Sheet, Plate, Welded Tube, Bar

0.15 %

Show Material materials with Titanium of 0.15 %

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

Zinc

0.15 %

Show Material materials with Zinc of 0.15 %

H14

EN 573-3, EN 1301, EN 1592, EN 485, EN 754

Rod, Flat, Seamless Tube, Tube, Wire, Strip, Sheet, Plate, Welded Tube, Bar

0.15 %

Show Material materials with Zinc of 0.15 %

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

Technological properties

Property
Anodizing

decorative: sufficient, Protective: very good

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Tubes: Industrial tubes, Pipes; Wind energy: Nacelle coverings, rotor hub, stairs;

Brazing

hard brazing (with flux/ without flux): sufficient / poor, friction soldering: good, soft brazing with flux: sufficient

Corrosion properties

Seawater: good, weathering: very good

Welding

Very Good

Workability

Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / acceptable (H12)