Naturally hard AlMg alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.68 g/cm³

Show Material materials with Density of 2.68 g/cm³

H46

EN 573-3, EN 1396

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

20.0 °C

2.68 g/cm³

Show Material materials with Density of 2.68 g/cm³

H46

EN 573-3

Sheet, Strip

20.0 °C

2.68 - 2.69 g/cm³

Show Material materials with Density of 2.68 - 2.69 g/cm³

H46

EN 573-3

Sheet, Strip

20.0 °C

2.69 g/cm³

Show Material materials with Density of 2.69 g/cm³

H46

EN 573-3

Sheet, Strip

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H46

EN 573-3, EN 1396

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H46

EN 573-3

Sheet, Strip

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

H46

EN 573-3

Sheet, Strip

Shear modulus

26.3 GPa

Show Material materials with Shear modulus of 26.3 GPa

H46

EN 573-3, EN 1396

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

20.0 °C

26.3 - 26.5 GPa

Show Material materials with Shear modulus of 26.3 - 26.5 GPa

H46

EN 573-3

Sheet, Strip

20.0 °C

26.3 GPa

Show Material materials with Shear modulus of 26.3 GPa

H46

EN 573-3

Sheet, Strip

Tensile strength

20.0 °C

210.0 - 270.0 MPa

Show Material materials with Tensile strength of 210.0 - 270.0 MPa

H46

EN 573-3

Sheet, Strip

Transverse

20.0 °C

210.0 - 270.0 MPa

Show Material materials with Tensile strength of 210.0 - 270.0 MPa

H46

EN 573-3, EN 1396

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.3699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3699999999999997e-05 1/K

H46

EN 573-3, EN 1396

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

100 °C

2.3699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3699999999999997e-05 1/K

H46

EN 573-3, EN 1396

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

610.0 - 650.0 °C

Show Material materials with Melting point of 610.0 - 650.0 °C

H46

EN 573-3, EN 1396

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

Specific heat capacity

20.0 °C

898.0 - 921.0 J/(kg·K)

Show Material materials with Specific heat capacity of 898.0 - 921.0 J/(kg·K)

H46

EN 573-3

Sheet, Strip

20.0 °C

898.0 J/(kg·K)

Show Material materials with Specific heat capacity of 898.0 J/(kg·K)

H46

EN 573-3

Sheet, Strip

20.0 °C

921.0 J/(kg·K)

Show Material materials with Specific heat capacity of 921.0 J/(kg·K)

H46

EN 573-3

Sheet, Strip

Thermal conductivity

140.0 - 160.0 W/(m·K)

Show Material materials with Thermal conductivity of 140.0 - 160.0 W/(m·K)

H46

EN 573-3, EN 1396

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

20.0 °C

149.0 - 167.0 W/(m·K)

Show Material materials with Thermal conductivity of 149.0 - 167.0 W/(m·K)

H46

EN 573-3

Sheet, Strip

20.0 °C

149.0 W/(m·K)

Show Material materials with Thermal conductivity of 149.0 W/(m·K)

H46

EN 573-3

Sheet, Strip

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

25000000.0 - 30000000.0 S/m

Show Material materials with Electrical conductivity of 25000000.0 - 30000000.0 S/m

H46

EN 573-3, EN 1396

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

20.0 °C

26000000.0 S/m

Show Material materials with Electrical conductivity of 26000000.0 S/m

H46

EN 573-3

Sheet, Strip

Electrical resistivity

3.33e-08 - 4e-08 Ω·m

Show Material materials with Electrical resistivity of 3.33e-08 - 4e-08 Ω·m

H46

EN 573-3, EN 1396

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

20.0 °C

4.6e-08 Ω·m

Show Material materials with Electrical resistivity of 4.6e-08 Ω·m

H46

EN 573-3

Sheet, Strip

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.15 %

Show Material materials with Chromium of 0.15 %

H46

EN 573-3, EN 1396

Sheet, Strip, Plate, Wire, Tube, Welded Tube, Bar

Copper

0.15 %

Show Material materials with Copper of 0.15 %

H46

EN 573-3, EN 1396

Sheet, Strip, Plate, Wire, Tube, Welded Tube, Bar

Iron

0.5 %

Show Material materials with Iron of 0.5 %

H46

EN 573-3

Sheet, Strip

0.50 %

Show Material materials with Iron of 0.50 %

H46

EN 573-3, EN 1396

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

Magnesium

1.7 - 2.4 %

Show Material materials with Magnesium of 1.7 - 2.4 %

H46

EN 573-3, EN 1396

Sheet, Strip, Plate, Wire, Tube, Welded Tube, Bar

Manganese

0.1 - 0.5 %

Show Material materials with Manganese of 0.1 - 0.5 %

H46

EN 573-3, EN 1396

Sheet, Strip, Plate, Wire, Tube, Welded Tube, Bar

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

H46

EN 573-3, EN 1396

Sheet, Strip, Plate, Wire, Tube, Welded Tube, Bar

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

H46

EN 573-3, EN 1396

Sheet, Strip, Plate, Wire, Tube, Welded Tube, Bar

Zinc

0.15 %

Show Material materials with Zinc of 0.15 %

H46

EN 573-3, EN 1396

Sheet, Strip, Plate, Wire, Tube, Welded Tube, Bar

Technological properties

Property
Anodizing

decorative: sufficient, Protective: very good

Brazing

hard brazing (with flux/ without flux): sufficient / poor, friction soldering: good, soft brazing with flux: sufficient

Corrosion properties

Seawater: good, weathering: very good

Workability

Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / acceptable (H12)