EN 573-3 Grade AW-5251 O

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlMg alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey,Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.68 g/cm³

Show Material materials with Density of 2.68 g/cm³

O

EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

20.0 °C

2.68 g/cm³

Show Material materials with Density of 2.68 g/cm³

O

EN 573-3

Sheet, Strip, Rod, Flat, Tube, Wire

20.0 °C

2.68 - 2.69 g/cm³

Show Material materials with Density of 2.68 - 2.69 g/cm³

O

EN 573-3

Sheet, Strip, Rod, Flat, Tube, Wire

20.0 °C

2.69 g/cm³

Show Material materials with Density of 2.69 g/cm³

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3

Coil, Sheet, Plate, Strip, Sheet, Strip, Rod, Flat, Tube, Wire

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.2 mm

Show Material materials with Thickness of 0.2 mm

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

0.2 mm

Coil, Sheet, Plate, Strip

6.0 mm

Show Material materials with Thickness of 6.0 mm

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

6.0 mm

Coil, Sheet, Plate, Strip

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

100.0 MPa

Show Material materials with Bending Fatigue Strength of 100.0 MPa

O

EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

Bending angle 180°

0 °/t

Show Material materials with Bending angle 180° of 0 °/t

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

0.5 °/t

Show Material materials with Bending angle 180° of 0.5 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

0.5 °/t

Show Material materials with Bending angle 180° of 0.5 °/t

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

Bending angle 90°

0 °/t

Show Material materials with Bending angle 90° of 0 °/t

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

2.0 °/t

Show Material materials with Bending angle 90° of 2.0 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

2.0 °/t

Show Material materials with Bending angle 90° of 2.0 °/t

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

Elastic modulus

68.6 GPa

Show Material materials with Elastic modulus of 68.6 GPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

O

EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

O

EN 573-3

Sheet, Strip, Rod, Flat, Tube, Wire

Elongation

13.0 %

Show Material materials with Elongation of 13.0 %

O

EN 573-3, EN 1396, EN 485

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

A50

13.0 - 18.0 %

Show Material materials with Elongation of 13.0 - 18.0 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

A50

14.0 %

Show Material materials with Elongation of 14.0 %

O

EN 573-3, EN 1396, EN 485

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

A50

15.0 %

Show Material materials with Elongation of 15.0 %

O

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

A50

15.0 %

Show Material materials with Elongation of 15.0 %

O

EN 573-3, EN 1301

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

16.0 %

Show Material materials with Elongation of 16.0 %

O

EN 573-3, EN 1396, EN 485

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

A50

17.0 %

Show Material materials with Elongation of 17.0 %

O

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

A100

18.0 %

Show Material materials with Elongation of 18.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

A50

18.0 %

Show Material materials with Elongation of 18.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

A100

20.0 °C

13.0 %

Show Material materials with Elongation of 13.0 %

O

EN 573-3

Sheet, Strip, Flat

A50 Transverse

20.0 °C

13.0 %

Show Material materials with Elongation of 13.0 %

O

EN 573-3

Sheet, Strip, Flat

A50

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

O

EN 573-3

Sheet, Strip, Flat

A50 Transverse

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

O

EN 573-3

Sheet, Strip, Flat

A50

20.0 °C

15.0 %

Show Material materials with Elongation of 15.0 %

O

EN 573-3

Rod, Tube

A50

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

O

EN 573-3

Sheet, Strip, Flat

A50 Transverse

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

O

EN 573-3

Sheet, Strip, Flat

A50

20.0 °C

17.0 %

Show Material materials with Elongation of 17.0 %

O

EN 573-3

Rod, Tube

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

O

EN 573-3

Flat

A50

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

O

EN 573-3

Flat

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

O

EN 573-3

Flat

Transverse

Hardness, Brinell

44.0 [-]

Show Material materials with Hardness, Brinell of 44.0 [-]

O

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

20.0 °C

44.0 [-]

Show Material materials with Hardness, Brinell of 44.0 [-]

O

EN 573-3

Flat

20.0 °C

45.0 [-]

Show Material materials with Hardness, Brinell of 45.0 [-]

O

EN 573-3

Rod, Tube

Hardness, HBW

44 [-]

Show Material materials with Hardness, HBW of 44 [-]

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

O

EN 573-3

Sheet, Strip, Rod, Flat, Tube, Wire

Shear modulus

26.3 GPa

Show Material materials with Shear modulus of 26.3 GPa

O

EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

20.0 °C

26.3 - 26.5 GPa

Show Material materials with Shear modulus of 26.3 - 26.5 GPa

O

EN 573-3

Sheet, Strip, Rod, Flat, Tube, Wire

20.0 °C

26.3 GPa

Show Material materials with Shear modulus of 26.3 GPa

O

EN 573-3

Sheet, Strip, Rod, Flat, Tube, Wire

Tensile strength

215.0 MPa

Show Material materials with Tensile strength of 215.0 MPa

O

EN 573-3, EN 1301

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

20.0 °C

150.0 - 200.0 MPa

Show Material materials with Tensile strength of 150.0 - 200.0 MPa

O

EN 573-3, EN 754

Rod, Tube, Strip, Sheet, Plate, Wire, Welded Tube, Bar

20.0 °C

160.0 - 200.0 MPa

Show Material materials with Tensile strength of 160.0 - 200.0 MPa

O

EN 573-3

Sheet, Strip, Flat

Transverse

20.0 °C

160.0 - 220.0 MPa

Show Material materials with Tensile strength of 160.0 - 220.0 MPa

O

EN 573-3, EN 755

Rod, Tube, Strip, Sheet, Plate, Wire, Welded Tube, Bar

20.0 °C

160.0 - 200.0 MPa

Show Material materials with Tensile strength of 160.0 - 200.0 MPa

O

EN 573-3, EN 1396, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Flat, Plate, Wire, Tube, Welded Tube, Bar, Coil, Sheet, Plate, Strip

Yield strength

60.0 MPa

Show Material materials with Yield strength of 60.0 MPa

O

EN 573-3, EN 1396, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

RP02

60 MPa

Show Material materials with Yield strength of 60 MPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

95.0 MPa

Show Material materials with Yield strength of 95.0 MPa

O

EN 573-3, EN 1301

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

RP02

20.0 °C

60.0 MPa

Show Material materials with Yield strength of 60.0 MPa

O

EN 573-3

Sheet, Strip, Flat

RP02 Transverse

20.0 °C

60.0 MPa

Show Material materials with Yield strength of 60.0 MPa

O

EN 573-3

Rod, Tube, Sheet, Strip, Flat

RP02

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.3699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3699999999999997e-05 1/K

O

EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

100 °C

2.3699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3699999999999997e-05 1/K

O

EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

20-100°C

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

610.0 - 650.0 °C

Show Material materials with Melting point of 610.0 - 650.0 °C

O

EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

Specific heat capacity

20.0 °C

898.0 - 921.0 J/(kg·K)

Show Material materials with Specific heat capacity of 898.0 - 921.0 J/(kg·K)

O

EN 573-3

Sheet, Strip, Rod, Flat, Tube, Wire

20.0 °C

898.0 J/(kg·K)

Show Material materials with Specific heat capacity of 898.0 J/(kg·K)

O

EN 573-3

Sheet, Strip, Rod, Flat, Tube, Wire

20.0 °C

921.0 J/(kg·K)

Show Material materials with Specific heat capacity of 921.0 J/(kg·K)

O

EN 573-3

Sheet, Strip, Rod, Flat, Tube, Wire

Thermal conductivity

140.0 - 160.0 W/(m·K)

Show Material materials with Thermal conductivity of 140.0 - 160.0 W/(m·K)

O

EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

153 W/(m·K)

Show Material materials with Thermal conductivity of 153 W/(m·K)

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

20.0 °C

149.0 - 167.0 W/(m·K)

Show Material materials with Thermal conductivity of 149.0 - 167.0 W/(m·K)

O

EN 573-3

Sheet, Strip, Rod, Flat, Tube, Wire

20.0 °C

149.0 W/(m·K)

Show Material materials with Thermal conductivity of 149.0 W/(m·K)

O

EN 573-3

Sheet, Strip, Rod, Flat, Tube, Wire

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

25000000.0 - 30000000.0 S/m

Show Material materials with Electrical conductivity of 25000000.0 - 30000000.0 S/m

O

EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

20.0 °C

26000000.0 S/m

Show Material materials with Electrical conductivity of 26000000.0 S/m

O

EN 573-3

Sheet, Strip, Rod, Flat, Tube, Wire

Electrical resistivity

3.33e-08 - 4e-08 Ω·m

Show Material materials with Electrical resistivity of 3.33e-08 - 4e-08 Ω·m

O

EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

4.5e-08 Ω·m

Show Material materials with Electrical resistivity of 4.5e-08 Ω·m

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

20.0 °C

4.6e-08 Ω·m

Show Material materials with Electrical resistivity of 4.6e-08 Ω·m

O

EN 573-3

Sheet, Strip, Rod, Flat, Tube, Wire

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.15 %

Show Material materials with Chromium of 0.15 %

O

EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755

Sheet, Strip, Rod, Flat, Tube, Wire, Plate, Welded Tube, Bar

0.15 %

Show Material materials with Chromium of 0.15 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

Copper

0.15 %

Show Material materials with Copper of 0.15 %

O

EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755

Sheet, Strip, Rod, Flat, Tube, Wire, Plate, Welded Tube, Bar

0.15 %

Show Material materials with Copper of 0.15 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

Iron

0.5 %

Show Material materials with Iron of 0.5 %

O

EN 573-3

Sheet, Strip, Rod, Flat, Tube, Wire

0.50 %

Show Material materials with Iron of 0.50 %

O

EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar

0.5 %

Show Material materials with Iron of 0.5 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

Magnesium

1.7 - 2.4 %

Show Material materials with Magnesium of 1.7 - 2.4 %

O

EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Rod, Flat, Tube, Wire, Plate, Welded Tube, Bar, Coil, Sheet, Plate, Strip

Manganese

0.1 - 0.5 %

Show Material materials with Manganese of 0.1 - 0.5 %

O

EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Rod, Flat, Tube, Wire, Plate, Welded Tube, Bar, Coil, Sheet, Plate, Strip

Other

0.05 - 0.15 %

Show Material materials with Other of 0.05 - 0.15 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

O

EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755

Sheet, Strip, Rod, Flat, Tube, Wire, Plate, Welded Tube, Bar

0.4 %

Show Material materials with Silicon of 0.4 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

O

EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755

Sheet, Strip, Rod, Flat, Tube, Wire, Plate, Welded Tube, Bar

0.15 %

Show Material materials with Titanium of 0.15 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

Zinc

0.15 %

Show Material materials with Zinc of 0.15 %

O

EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755

Sheet, Strip, Rod, Flat, Tube, Wire, Plate, Welded Tube, Bar

0.15 %

Show Material materials with Zinc of 0.15 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate, Strip

Technological properties

Property
Anodizing

decorative: sufficient, Protective: very good

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Tubes: Industrial tubes, Pipes; Wind energy: Nacelle coverings, rotor hub, stairs;

Brazing

hard brazing (with flux/ without flux): sufficient / poor, friction soldering: good, soft brazing with flux: sufficient

Corrosion properties

Seawater: good, weathering: very good

Welding

Very Good

Workability

Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / acceptable (H12)