EN 573-3 Grade AW-5383 H321

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlMg alloy. The alloy is not food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated StandardsShape

Density

2.66 g/cm³

Show Material materials with Density of 2.66 g/cm³

H321

EN 573-3, EN 13195, EN 485

Strip, Sheet, Plate

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending angle 180°

3.0 °/t

Show Material materials with Bending angle 180° of 3.0 °/t

H321

EN 573-3, EN 485

Strip, Sheet, Plate

Unlock all property charts

Bending angle 90°

2.0 °/t

Show Material materials with Bending angle 90° of 2.0 °/t

H321

EN 573-3, EN 485

Strip, Sheet, Plate

2.5 °/t

Show Material materials with Bending angle 90° of 2.5 °/t

H321

EN 573-3, EN 485

Strip, Sheet, Plate

4.0 °/t

Show Material materials with Bending angle 90° of 4.0 °/t

H321

EN 573-3, EN 485

Strip, Sheet, Plate

Unlock all property charts

Elastic modulus

69.0 - 70.0 GPa

Show Material materials with Elastic modulus of 69.0 - 70.0 GPa

Typical for Wrought 5000 Series Aluminium

Unlock all property charts

Elongation

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

H321

EN 573-3

Flat

Transverse

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

H321

EN 573-3

Sheet, Flat

10.0 %

Show Material materials with Elongation of 10.0 %

H321

EN 573-3, EN 485

Strip, Sheet, Plate

Unlock all property charts

Elongation A50

20.0 °C

8 - 12 %

Show Material materials with Elongation A50 of 8 - 12 %

23.0 °C

8 - 10 %

Show Material materials with Elongation A50 of 8 - 10 %

Unlock all property charts

Elongation A50, transverse

20.0 °C

8 - 10 %

Show Material materials with Elongation A50, transverse of 8 - 10 %

Elongation, transverse

20.0 °C

10 %

Show Material materials with Elongation, transverse of 10 %

Hardness, Brinell

20.0 °C

84.0 [-]

Show Material materials with Hardness, Brinell of 84.0 [-]

H321

EN 573-3

Sheet, Flat

20.0 °C

90.0 [-]

Show Material materials with Hardness, Brinell of 90.0 [-]

H321

EN 573-3

Flat

20.0 °C

84.0 - 90.0 [-]

Show Material materials with Hardness, Brinell of 84.0 - 90.0 [-]

H321

EN 573-3

Flat

90.0 [-]

Show Material materials with Hardness, Brinell of 90.0 [-]

H321

EN 573-3, EN 485

Strip, Sheet, Plate

84.0 [-]

Show Material materials with Hardness, Brinell of 84.0 [-]

H321

EN 573-3, EN 485

Strip, Sheet, Plate

Unlock all property charts

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Unlock all property charts

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 5000 Series Aluminium

Unlock all property charts

Shear modulus

26.0 - 26.5 GPa

Show Material materials with Shear modulus of 26.0 - 26.5 GPa

Typical for Wrought 5000 Series Aluminium

Unlock all property charts

Tensile strength

20.0 °C

330.0 - 400.0 MPa

Show Material materials with Tensile strength of 330.0 - 400.0 MPa

H321

EN 573-3

Flat

Transverse

20.0 °C

285.0 MPa

Show Material materials with Tensile strength of 285.0 MPa

H321

EN 573-3

Sheet

20.0 °C

305.0 MPa

Show Material materials with Tensile strength of 305.0 MPa

H321

EN 573-3

Flat

330.0 - 400.0 MPa

Show Material materials with Tensile strength of 330.0 - 400.0 MPa

H321

EN 573-3, EN 485

Strip, Sheet, Plate

Unlock all property charts

Tensile strength, transverse

20.0 °C

330 - 400 MPa

Show Material materials with Tensile strength, transverse of 330 - 400 MPa

Yield strength Rp0.2

20.0 °C

205 - 220 MPa

Show Material materials with Yield strength Rp0.2 of 205 - 220 MPa

23.0 °C

230 MPa

Show Material materials with Yield strength Rp0.2 of 230 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

230 MPa

Show Material materials with Yield strength Rp0.2, transverse of 230 MPa

Thermal

PropertyValueComment

Coefficient of thermal expansion

2.2e-05 - 2.5e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2e-05 - 2.5e-05 1/K

Typical for Wrought 5000 Series Aluminium

Unlock all property charts

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

560.0 - 655.0 °C

Show Material materials with Melting point of 560.0 - 655.0 °C

Typical for Wrought 5000 Series Aluminium

Specific heat capacity

879.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 879.0 - 963.0 J/(kg·K)

Typical for Wrought 5000 Series Aluminium

Unlock all property charts

Thermal conductivity

112.0 - 205.0 W/(m·K)

Show Material materials with Thermal conductivity of 112.0 - 205.0 W/(m·K)

Typical for Wrought 5000 Series Aluminium

Unlock all property charts

Electrical

PropertyValueComment

Electrical conductivity

18000000.0 - 31000000.0 S/m

Show Material materials with Electrical conductivity of 18000000.0 - 31000000.0 S/m

Typical for Wrought 5000 Series Aluminium

Unlock all property charts

Electrical resistivity

3.3e-08 - 5e-08 Ω·m

Show Material materials with Electrical resistivity of 3.3e-08 - 5e-08 Ω·m

Typical for Wrought 5000 Series Aluminium

Unlock all property charts

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.25 %

Show Material materials with Chromium of 0.25 %

H321

EN 573-3, EN 13195, EN 485

Flat, Sheet, Strip, Plate

Copper

0.2 %

Show Material materials with Copper of 0.2 %

H321

EN 573-3, EN 13195, EN 485

Flat, Sheet, Strip, Plate

Iron

0.25 %

Show Material materials with Iron of 0.25 %

H321

EN 573-3

Flat, Sheet

0.25 %

Show Material materials with Iron of 0.25 %

H321

EN 573-3, EN 13195, EN 485

Strip, Sheet, Plate

Magnesium

4.0 - 5.2 %

Show Material materials with Magnesium of 4.0 - 5.2 %

H321

EN 573-3, EN 13195, EN 485

Flat, Sheet, Strip, Plate

Manganese

0.7 - 1.0 %

Show Material materials with Manganese of 0.7 - 1.0 %

H321

EN 573-3, EN 13195, EN 485

Flat, Sheet, Strip, Plate

Other

each 0.05, total 0.15, Rest Al

Silicon

0.25 %

Show Material materials with Silicon of 0.25 %

H321

EN 573-3, EN 13195, EN 485

Flat, Sheet, Strip, Plate

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

H321

EN 573-3, EN 13195, EN 485

Flat, Sheet, Strip, Plate

Zinc

0.4 %

Show Material materials with Zinc of 0.4 %

H321

EN 573-3, EN 13195, EN 485

Flat, Sheet, Strip, Plate

Zirconium

0.2 %

Show Material materials with Zirconium of 0.2 %

H321

EN 573-3, EN 13195, EN 485

Flat, Sheet, Strip, Plate

Technological properties

Property
Workability

Good workability.