General
Property | Value | Temperature |
---|---|---|
Density | 2.66 g/cm³ Show Material materials with Density of 2.66 g/cm³ at 23.0 °C | 23.0 °C |
Mechanical
Property | Value | Temperature | Comment |
---|---|---|---|
Bending angle 90° | 1 - 4.5 °/t Show Material materials with Bending angle 90° of 1 - 4.5 °/t at 23.0 °C | 23.0 °C | |
Elastic modulus | 69 - 70 GPa Show Material materials with Elastic modulus of 69 - 70 GPa at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Elongation | 7 % Show Material materials with Elongation of 7 % at 20.0 °C | 20.0 °C | |
Elongation A100 | 7 % Show Material materials with Elongation A100 of 7 % at 23.0 °C | 23.0 °C | |
Elongation A50 | 4 - 8 % Show Material materials with Elongation A50 of 4 - 8 % at 20.0 °C | 20.0 °C | |
4 - 8 % Show Material materials with Elongation A50 of 4 - 8 % at 23.0 °C | 23.0 °C | ||
Elongation A50, transverse | 4 - 8 % Show Material materials with Elongation A50, transverse of 4 - 8 % at 20.0 °C | 20.0 °C | |
Elongation, transverse | 7 % Show Material materials with Elongation, transverse of 7 % at 20.0 °C | 20.0 °C | |
Hardness, Brinell | 105 [-] Show Material materials with Hardness, Brinell of 105 [-] at 20.0 °C | 20.0 °C | |
105 [-] Show Material materials with Hardness, Brinell of 105 [-] at 23.0 °C | 23.0 °C | ||
Plane-Strain Fracture Toughnes | 22 - 35 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Shear modulus | 26 - 26.5 GPa Show Material materials with Shear modulus of 26 - 26.5 GPa at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Shear strength | 105 MPa Show Material materials with Shear strength of 105 MPa at 20.0 °C | 20.0 °C | |
Tensile strength | 340 - 400 MPa Show Material materials with Tensile strength of 340 - 400 MPa at 20.0 °C | 20.0 °C | |
340 - 400 MPa Show Material materials with Tensile strength of 340 - 400 MPa at 23.0 °C | 23.0 °C | ||
Tensile strength, transverse | 340 - 400 MPa Show Material materials with Tensile strength, transverse of 340 - 400 MPa at 20.0 °C | 20.0 °C | |
Yield strength Rp0.2 | 270 MPa Show Material materials with Yield strength Rp0.2 of 270 MPa at 20.0 °C | 20.0 °C | |
270 MPa Show Material materials with Yield strength Rp0.2 of 270 MPa at 23.0 °C | 23.0 °C | ||
Yield strength Rp0.2, transverse | 270 MPa Show Material materials with Yield strength Rp0.2, transverse of 270 MPa at 20.0 °C | 20.0 °C |
Thermal
Property | Value | Temperature | Comment |
---|---|---|---|
Coefficient of thermal expansion | 2.2E-5 - 2.5E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.2E-5 - 2.5E-5 1/K at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Max service temperature | 150 °C Show Material materials with Max service temperature of 150 °C | Typical for Wrought 5000 Series Aluminium | |
Melting point | 560 - 655 °C Show Material materials with Melting point of 560 - 655 °C | Typical for Wrought 5000 Series Aluminium | |
Specific heat capacity | 879 - 963 J/(kg·K) Show Material materials with Specific heat capacity of 879 - 963 J/(kg·K) at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Thermal conductivity | 112 - 205 W/(m·K) Show Material materials with Thermal conductivity of 112 - 205 W/(m·K) at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Electrical
Property | Value | Temperature | Comment |
---|---|---|---|
Electrical conductivity | 1.80E+7 - 3.10E+7 S/m Show Material materials with Electrical conductivity of 1.80E+7 - 3.10E+7 S/m at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Electrical resistivity | 3.3E-8 - 5E-8 Ω·m Show Material materials with Electrical resistivity of 3.3E-8 - 5E-8 Ω·m at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Chemical properties
Property | ||
---|---|---|
Chromium | 0.25 % | |
Copper | 0.2 % | |
Iron | 0.25 % | |
Magnesium | 4 - 5.2 % | |
Manganese | 0.7 - 1 % | |
Other | each 0.05, total 0.15, Rest Al | |
Silicon | 0.25 % | |
Titanium | 0.15 % | |
Zinc | 0.4 % | |
Zirconium | 0.2 % |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |