EN 573-3 Grade AW-5754 F

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlMg alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.66 g/cm³

Show Material materials with Density of 2.66 g/cm³

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

20.0 °C

2.66 g/cm³

Show Material materials with Density of 2.66 g/cm³

F

EN 573-3

Profile, Rod, Flat, Tube, Sheet, Plate

20.0 °C

2.66 - 2.68 g/cm³

Show Material materials with Density of 2.66 - 2.68 g/cm³

F

EN 573-3

Profile, Rod, Flat, Tube, Sheet, Plate

20.0 °C

2.68 g/cm³

Show Material materials with Density of 2.68 g/cm³

F

EN 573-3

Profile, Rod, Flat, Tube, Sheet, Plate

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

-270.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Sheet, Plate

70.5 GPa

Show Material materials with Elastic modulus of 70.5 GPa

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Sheet, Plate

20.0 °C

70.0 - 70.5 GPa

Show Material materials with Elastic modulus of 70.0 - 70.5 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Sheet, Plate

20.0 °C

70.5 GPa

Show Material materials with Elastic modulus of 70.5 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Sheet, Plate

50.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube

100.0 °C

68.0 GPa

Show Material materials with Elastic modulus of 68.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube

150.0 °C

66.0 GPa

Show Material materials with Elastic modulus of 66.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube

200.0 °C

63.0 GPa

Show Material materials with Elastic modulus of 63.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube

250.0 °C

57.0 GPa

Show Material materials with Elastic modulus of 57.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube

300.0 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube

Elongation

12.0 %

Show Material materials with Elongation of 12.0 %

F

EN 573-3, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A50

14.0 %

Show Material materials with Elongation of 14.0 %

F

EN 573-3, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A100

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

F

EN 573-3

Profile, Rod, Tube

A50

20.0 °C

13.0 %

Show Material materials with Elongation of 13.0 %

F

EN 573-3

Rod

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

F

EN 573-3

Profile, Tube, Rod

20.0 °C

23.0 %

Show Material materials with Elongation of 23.0 %

F

EN 573-3

60.0 °C

22.0 %

Show Material materials with Elongation of 22.0 %

F

EN 573-3

100.0 °C

21.0 %

Show Material materials with Elongation of 21.0 %

F

EN 573-3

140.0 °C

38.0 %

Show Material materials with Elongation of 38.0 %

F

EN 573-3

180.0 °C

38.0 %

Show Material materials with Elongation of 38.0 %

F

EN 573-3

240.0 °C

47.0 %

Show Material materials with Elongation of 47.0 %

F

EN 573-3

300.0 °C

66.0 %

Show Material materials with Elongation of 66.0 %

F

EN 573-3

360.0 °C

102.0 %

Show Material materials with Elongation of 102.0 %

F

EN 573-3

Hardness, Brinell

58.0 [-]

Show Material materials with Hardness, Brinell of 58.0 [-]

F

EN 573-3, EN 570

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

20.0 °C

47.0 [-]

Show Material materials with Hardness, Brinell of 47.0 [-]

F

EN 573-3

Profile, Tube, Rod

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

F

EN 573-3

Profile, Rod, Flat, Tube, Sheet, Plate

Shear modulus

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

20.0 °C

26.5 - 27.0 GPa

Show Material materials with Shear modulus of 26.5 - 27.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Sheet, Plate

20.0 °C

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Sheet, Plate

Tensile strength

180.0 MPa

Show Material materials with Tensile strength of 180.0 MPa

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

190.0 - 250.0 MPa

Show Material materials with Tensile strength of 190.0 - 250.0 MPa

F

EN 573-3, EN 1715-3, EN 1715-4

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

190.0 MPa

Show Material materials with Tensile strength of 190.0 MPa

F

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

20.0 °C

180.0 MPa

Show Material materials with Tensile strength of 180.0 MPa

F

EN 573-3

Profile, Tube, Sheet, Rod

20.0 °C

180.0 MPa

Show Material materials with Tensile strength of 180.0 MPa

F

EN 573-3

Flat

Transverse

20.0 °C

190.0 MPa

Show Material materials with Tensile strength of 190.0 MPa

F

EN 573-3

Flat

20.0 °C

190.0 MPa

Show Material materials with Tensile strength of 190.0 MPa

F

EN 573-3

Flat

Transverse

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.3899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3899999999999998e-05 1/K

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

100 °C

2.3899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3899999999999998e-05 1/K

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

100.0 °C

2.39e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.39e-05 1/K

F

EN 573-3

Profile, Rod, Flat, Tube, Sheet, Plate

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

610.0 - 640.0 °C

Show Material materials with Melting point of 610.0 - 640.0 °C

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

Specific heat capacity

20.0 °C

897.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 897.0 - 963.0 J/(kg·K)

F

EN 573-3

Profile, Rod, Flat, Tube, Sheet, Plate

20.0 °C

897.0 J/(kg·K)

Show Material materials with Specific heat capacity of 897.0 J/(kg·K)

F

EN 573-3

Profile, Rod, Flat, Tube, Sheet, Plate

20.0 °C

963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 963.0 J/(kg·K)

F

EN 573-3

Profile, Rod, Flat, Tube, Sheet, Plate

Thermal conductivity

20.0 °C

132.0 - 160.0 W/(m·K)

Show Material materials with Thermal conductivity of 132.0 - 160.0 W/(m·K)

F

EN 573-3

Profile, Rod, Flat, Tube, Sheet, Plate

20.0 °C

132.0 - 140.0 W/(m·K)

Show Material materials with Thermal conductivity of 132.0 - 140.0 W/(m·K)

F

EN 573-3

Profile, Rod, Flat, Tube, Sheet, Plate

20.0 °C

132.0 W/(m·K)

Show Material materials with Thermal conductivity of 132.0 W/(m·K)

F

EN 573-3

Profile, Rod, Flat, Tube, Sheet, Plate

20.0 °C

140.0 - 160.0 W/(m·K)

Show Material materials with Thermal conductivity of 140.0 - 160.0 W/(m·K)

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Profile, Rod, Flat

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

20000000.0 - 23000000.0 S/m

Show Material materials with Electrical conductivity of 20000000.0 - 23000000.0 S/m

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Profile, Rod, Flat

Electrical resistivity

4.35e-08 - 5e-08 Ω·m

Show Material materials with Electrical resistivity of 4.35e-08 - 5e-08 Ω·m

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

20.0 °C

4.3e-08 - 5.3e-08 Ω·m

Show Material materials with Electrical resistivity of 4.3e-08 - 5.3e-08 Ω·m

F

EN 573-3

Profile, Rod, Flat, Tube, Sheet, Plate

20.0 °C

4.3e-08 - 5e-08 Ω·m

Show Material materials with Electrical resistivity of 4.3e-08 - 5e-08 Ω·m

F

EN 573-3

Profile, Rod, Flat, Tube, Sheet, Plate

20.0 °C

5e-08 - 5.3e-08 Ω·m

Show Material materials with Electrical resistivity of 5e-08 - 5.3e-08 Ω·m

F

EN 573-3

Profile, Rod, Flat, Tube, Sheet, Plate

20.0 °C

5.3e-08 Ω·m

Show Material materials with Electrical resistivity of 5.3e-08 Ω·m

F

EN 573-3

Profile, Rod, Flat, Tube, Sheet, Plate

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.3 %

Show Material materials with Chromium of 0.3 %

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Profile, Rod, Flat, Tube, Sheet, Plate, Strip, Wire, Forging, Bar

Copper

0.1 %

Show Material materials with Copper of 0.1 %

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Profile, Rod, Flat, Tube, Sheet, Plate, Strip, Wire, Forging, Bar

Iron

0.4 %

Show Material materials with Iron of 0.4 %

F

EN 573-3

Profile, Rod, Flat, Tube, Sheet, Plate

0.40 %

Show Material materials with Iron of 0.40 %

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

Magnesium

2.6 - 3.6 %

Show Material materials with Magnesium of 2.6 - 3.6 %

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Profile, Rod, Flat, Tube, Sheet, Plate, Strip, Wire, Forging, Bar

Manganese

0.5 %

Show Material materials with Manganese of 0.5 %

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Profile, Rod, Flat, Tube, Sheet, Plate, Strip, Wire, Forging, Bar

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Profile, Rod, Flat, Tube, Sheet, Plate, Strip, Wire, Forging, Bar

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Profile, Rod, Flat, Tube, Sheet, Plate, Strip, Wire, Forging, Bar

Zinc

0.2 %

Show Material materials with Zinc of 0.2 %

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Profile, Rod, Flat, Tube, Sheet, Plate, Strip, Wire, Forging, Bar

Technological properties

Property
Anodizing

decorative: gut (EQ: sehr gut), Protective: very good

Brazing

hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor

Corrosion properties

Seawater: very good to good, weathering: very good

Workability

Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12)