EN 573-3 Grade AW-5754 H111

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlMg alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey,Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.66 g/cm³

Show Material materials with Density of 2.66 g/cm³

H111

EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

2.67 g/cm³

Show Material materials with Density of 2.67 g/cm³

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

20.0 °C

2.66 g/cm³

Show Material materials with Density of 2.66 g/cm³

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

20.0 °C

2.66 - 2.68 g/cm³

Show Material materials with Density of 2.66 - 2.68 g/cm³

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

20.0 °C

2.68 g/cm³

Show Material materials with Density of 2.68 g/cm³

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

1.5 mm

Show Material materials with Thickness of 1.5 mm

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

1.5 mm

Sheet, Strip, Plate

3.0 mm

Show Material materials with Thickness of 3.0 mm

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

3.0 mm

Sheet, Strip, Plate

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending angle 180°

0.5 °/t

Show Material materials with Bending angle 180° of 0.5 °/t

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

1.0 °/t

Show Material materials with Bending angle 180° of 1.0 °/t

H111

EN 573-3, EN 14286, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

1 °/t

Show Material materials with Bending angle 180° of 1 °/t

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

2.0 °/t

Show Material materials with Bending angle 180° of 2.0 °/t

H111

EN 573-3, EN 14286

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

Bending angle 90°

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

1 °/t

Show Material materials with Bending angle 90° of 1 °/t

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

2.0 °/t

Show Material materials with Bending angle 90° of 2.0 °/t

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

Elastic modulus

-270 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H111

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Strip, Plate, Rod, Flat

-270.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H111

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Strip, Plate, Rod, Flat

70.5 GPa

Show Material materials with Elastic modulus of 70.5 GPa

H111

EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

20 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H111

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Strip, Plate, Rod, Flat

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H111

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Strip, Plate, Rod, Flat

20.0 °C

70.0 - 70.5 GPa

Show Material materials with Elastic modulus of 70.0 - 70.5 GPa

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

20.0 °C

70.5 GPa

Show Material materials with Elastic modulus of 70.5 GPa

H111

EN 573-3

Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Rod, Flat

50.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

100.0 °C

68.0 GPa

Show Material materials with Elastic modulus of 68.0 GPa

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

150.0 °C

66.0 GPa

Show Material materials with Elastic modulus of 66.0 GPa

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

200.0 °C

63.0 GPa

Show Material materials with Elastic modulus of 63.0 GPa

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

250.0 °C

57.0 GPa

Show Material materials with Elastic modulus of 57.0 GPa

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

300 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

H111

EN 573-3

Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Rod, Flat

300.0 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

H111

EN 573-3

Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Rod, Flat

Elongation

12.0 %

Show Material materials with Elongation of 12.0 %

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A50

12 %

Show Material materials with Elongation of 12 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

A50

14.0 %

Show Material materials with Elongation of 14.0 %

H111

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A50

15.0 %

Show Material materials with Elongation of 15.0 %

H111

EN 573-3, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A50

16.0 %

Show Material materials with Elongation of 16.0 %

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A50

16.0 %

Show Material materials with Elongation of 16.0 %

H111

EN 573-3

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

16.0 %

Show Material materials with Elongation of 16.0 %

H111

EN 573-3, EN 754

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A100

17.0 %

Show Material materials with Elongation of 17.0 %

H111

EN 573-3

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

17.0 %

Show Material materials with Elongation of 17.0 %

H111

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A100

18.0 %

Show Material materials with Elongation of 18.0 %

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A50

18.0 %

Show Material materials with Elongation of 18.0 %

H111

EN 573-3

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

19.0 %

Show Material materials with Elongation of 19.0 %

H111

EN 573-3, EN 14286

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A100

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

H111

EN 573-3

Plate, Strip, Sheet, Flat

A50

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

H111

EN 573-3

Flat

A50 Transverse

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

H111

EN 573-3

Tube, Rod, Plate, Strip, Sheet, Flat

A50

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

H111

EN 573-3

Flat

A50 Transverse

20.0 °C

15.0 %

Show Material materials with Elongation of 15.0 %

H111

EN 573-3

Tube, Rod

A50

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

H111

EN 573-3

Plate, Strip, Sheet, Flat

A50

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

H111

EN 573-3

Tube, Rod

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

H111

EN 573-3

Flat

A50 Transverse

20.0 °C

17.0 %

Show Material materials with Elongation of 17.0 %

H111

EN 573-3

Tube, Rod, Flat

20.0 °C

17.0 %

Show Material materials with Elongation of 17.0 %

H111

EN 573-3

Flat

Transverse

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

H111

EN 573-3

Plate, Strip, Sheet, Flat

A50

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

H111

EN 573-3

Sheet, Strip

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

H111

EN 573-3

Flat

A50 Transverse

Hardness, Brinell

52.0 [-]

Show Material materials with Hardness, Brinell of 52.0 [-]

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

20.0 °C

45.0 [-]

Show Material materials with Hardness, Brinell of 45.0 [-]

H111

EN 573-3

Tube, Rod

20.0 °C

52.0 [-]

Show Material materials with Hardness, Brinell of 52.0 [-]

H111

EN 573-3

Flat

Hardness, HBW

52 [-]

Show Material materials with Hardness, HBW of 52 [-]

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

Impact strength, Charpy notched

30.0 kJ/m²

Show Material materials with Impact strength, Charpy notched of 30.0 kJ/m²

H111

EN 573-3

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

Shear modulus

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

H111

EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

27.0 GPa

Show Material materials with Shear modulus of 27.0 GPa

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

20.0 °C

26.5 - 27.0 GPa

Show Material materials with Shear modulus of 26.5 - 27.0 GPa

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

20.0 °C

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

Tensile strength

180.0 MPa

Show Material materials with Tensile strength of 180.0 MPa

H111

EN 573-3

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

190.0 MPa

Show Material materials with Tensile strength of 190.0 MPa

H111

EN 573-3

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

20.0 °C

180.0 MPa

Show Material materials with Tensile strength of 180.0 MPa

H111

EN 573-3

Transverse

20.0 °C

180.0 - 250.0 MPa

Show Material materials with Tensile strength of 180.0 - 250.0 MPa

H111

EN 573-3, EN 754, EN 755

Tube, Rod, Strip, Sheet, Plate, Wire, Forging, Bar

20.0 °C

180.0 MPa

Show Material materials with Tensile strength of 180.0 MPa

H111

EN 573-3

Tube, Rod

20.0 °C

190.0 - 240.0 MPa

Show Material materials with Tensile strength of 190.0 - 240.0 MPa

H111

EN 573-3

Flat

Transverse

20.0 °C

190.0 MPa

Show Material materials with Tensile strength of 190.0 MPa

H111

EN 573-3

Sheet, Strip

20.0 °C

190.0 - 240.0 MPa

Show Material materials with Tensile strength of 190.0 - 240.0 MPa

H111

EN 573-3, EN 14286, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Flat, Strip, Plate

Yield strength

-270 °C

80.0 MPa

Show Material materials with Yield strength of 80.0 MPa

H111

EN 573-3

Tube, Rod, Sheet, Strip, Plate, Flat, Wire, Forging, Bar

RP02

-270.0 °C

80.0 MPa

Show Material materials with Yield strength of 80.0 MPa

H111

EN 573-3

Tube, Rod, Sheet, Strip, Plate, Flat, Wire, Forging, Bar

RP02

80.0 MPa

Show Material materials with Yield strength of 80.0 MPa

H111

EN 573-3, EN 14286, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

RP02

80 MPa

Show Material materials with Yield strength of 80 MPa

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

20.0 °C

80.0 MPa

Show Material materials with Yield strength of 80.0 MPa

H111

EN 573-3

Tube, Rod, Sheet, Strip, Plate, Flat, Wire, Forging, Bar

RP02

20 °C

80.0 MPa

Show Material materials with Yield strength of 80.0 MPa

H111

EN 573-3

Tube, Rod, Sheet, Strip, Plate, Flat, Wire, Forging, Bar

RP02

20.0 °C

80.0 MPa

Show Material materials with Yield strength of 80.0 MPa

H111

EN 573-3

Flat

RP02 Transverse

50.0 °C

80.0 MPa

Show Material materials with Yield strength of 80.0 MPa

H111

EN 573-3

Tube, Rod, Sheet, Strip, Plate, Flat, Wire, Forging, Bar

RP02

100 °C

70.0 MPa

Show Material materials with Yield strength of 70.0 MPa

H111

EN 573-3

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

RP02

100.0 °C

70.0 MPa

Show Material materials with Yield strength of 70.0 MPa

H111

EN 573-3

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

RP02

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.3899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3899999999999998e-05 1/K

H111

EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

100 °C

2.3899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3899999999999998e-05 1/K

H111

EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

100.0 °C

2.39e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.39e-05 1/K

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

20-100°C

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

610.0 - 640.0 °C

Show Material materials with Melting point of 610.0 - 640.0 °C

H111

EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

Specific heat capacity

20.0 °C

897.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 897.0 - 963.0 J/(kg·K)

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

20.0 °C

897.0 J/(kg·K)

Show Material materials with Specific heat capacity of 897.0 J/(kg·K)

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

20.0 °C

963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 963.0 J/(kg·K)

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

Thermal conductivity

147.0 - 168.0 W/(m·K)

Show Material materials with Thermal conductivity of 147.0 - 168.0 W/(m·K)

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

20.0 °C

132.0 - 160.0 W/(m·K)

Show Material materials with Thermal conductivity of 132.0 - 160.0 W/(m·K)

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

20.0 °C

132.0 - 140.0 W/(m·K)

Show Material materials with Thermal conductivity of 132.0 - 140.0 W/(m·K)

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

20.0 °C

132.0 W/(m·K)

Show Material materials with Thermal conductivity of 132.0 W/(m·K)

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

20.0 °C

140.0 - 160.0 W/(m·K)

Show Material materials with Thermal conductivity of 140.0 - 160.0 W/(m·K)

H111

EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Rod, Flat

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

20000000.0 - 23000000.0 S/m

Show Material materials with Electrical conductivity of 20000000.0 - 23000000.0 S/m

H111

EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Rod, Flat

Electrical resistivity

4.35e-08 - 5e-08 Ω·m

Show Material materials with Electrical resistivity of 4.35e-08 - 5e-08 Ω·m

H111

EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

4.9e-08 Ω·m

Show Material materials with Electrical resistivity of 4.9e-08 Ω·m

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

20.0 °C

4.3e-08 - 5.3e-08 Ω·m

Show Material materials with Electrical resistivity of 4.3e-08 - 5.3e-08 Ω·m

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

20.0 °C

4.3e-08 - 5e-08 Ω·m

Show Material materials with Electrical resistivity of 4.3e-08 - 5e-08 Ω·m

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

20.0 °C

5e-08 - 5.3e-08 Ω·m

Show Material materials with Electrical resistivity of 5e-08 - 5.3e-08 Ω·m

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

20.0 °C

5.3e-08 Ω·m

Show Material materials with Electrical resistivity of 5.3e-08 Ω·m

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.3 %

Show Material materials with Chromium of 0.3 %

H111

EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755

Tube, Plate, Strip, Sheet, Rod, Flat, Wire, Forging, Bar

0.3 %

Show Material materials with Chromium of 0.3 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

Copper

0.1 %

Show Material materials with Copper of 0.1 %

H111

EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755

Tube, Plate, Strip, Sheet, Rod, Flat, Wire, Forging, Bar

0.1 %

Show Material materials with Copper of 0.1 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

Iron

0.4 %

Show Material materials with Iron of 0.4 %

H111

EN 573-3

Tube, Plate, Strip, Sheet, Rod, Flat

0.40 %

Show Material materials with Iron of 0.40 %

H111

EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

0.4 %

Show Material materials with Iron of 0.4 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

Magnesium

2.6 - 3.6 %

Show Material materials with Magnesium of 2.6 - 3.6 %

H111

EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Tube, Plate, Strip, Sheet, Rod, Flat, Wire, Forging, Bar, Strip, Plate

Manganese

0.5 %

Show Material materials with Manganese of 0.5 %

H111

EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755

Tube, Plate, Strip, Sheet, Rod, Flat, Wire, Forging, Bar

0.5 %

Show Material materials with Manganese of 0.5 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

Other

0.1 - 0.6 %

Show Material materials with Other of 0.1 - 0.6 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

H111

EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755

Tube, Plate, Strip, Sheet, Rod, Flat, Wire, Forging, Bar

0.4 %

Show Material materials with Silicon of 0.4 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

H111

EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755

Tube, Plate, Strip, Sheet, Rod, Flat, Wire, Forging, Bar

0.15 %

Show Material materials with Titanium of 0.15 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

Zinc

0.2 %

Show Material materials with Zinc of 0.2 %

H111

EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755

Tube, Plate, Strip, Sheet, Rod, Flat, Wire, Forging, Bar

0.2 %

Show Material materials with Zinc of 0.2 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

Technological properties

Property
Anodizing

decorative: gut (EQ: sehr gut), Protective: very good

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Electronic devices: Housing of devices; Tubes: Industrial tubes, Pipes; Wind energy: Nacelle coverings, rotor hub, stairs; Components: Heat shields, Access hatches, Spoilers, Fuel and oil tanks, General transportation

Brazing

hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor

Corrosion properties

Seawater: very good to good, weathering: very good

Welding

Very Good

Workability

Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12)