EN 573-3 Grade AW-5754 H12

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlMg alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.66 g/cm³

Show Material materials with Density of 2.66 g/cm³

H12

EN 573-3, EN 1301, EN 1592, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

20.0 °C

2.66 g/cm³

Show Material materials with Density of 2.66 g/cm³

H12

EN 573-3

Wire, Flat, Seamless Tube

20.0 °C

2.66 - 2.68 g/cm³

Show Material materials with Density of 2.66 - 2.68 g/cm³

H12

EN 573-3

Wire, Flat, Seamless Tube

20.0 °C

2.68 g/cm³

Show Material materials with Density of 2.68 g/cm³

H12

EN 573-3

Wire, Flat, Seamless Tube

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

-270.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H12

EN 573-3

Wire, Flat, Seamless Tube

70.5 GPa

Show Material materials with Elastic modulus of 70.5 GPa

H12

EN 573-3, EN 1301, EN 1592, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H12

EN 573-3

Wire, Flat, Seamless Tube

20.0 °C

70.0 - 70.5 GPa

Show Material materials with Elastic modulus of 70.0 - 70.5 GPa

H12

EN 573-3

Wire, Flat, Seamless Tube

20.0 °C

70.5 GPa

Show Material materials with Elastic modulus of 70.5 GPa

H12

EN 573-3

Wire, Flat, Seamless Tube

50.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H12

EN 573-3

Wire, Flat, Seamless Tube

100.0 °C

68.0 GPa

Show Material materials with Elastic modulus of 68.0 GPa

H12

EN 573-3

Wire, Flat, Seamless Tube

150.0 °C

66.0 GPa

Show Material materials with Elastic modulus of 66.0 GPa

H12

EN 573-3

Wire, Flat, Seamless Tube

200.0 °C

63.0 GPa

Show Material materials with Elastic modulus of 63.0 GPa

H12

EN 573-3

Wire, Flat, Seamless Tube

250.0 °C

57.0 GPa

Show Material materials with Elastic modulus of 57.0 GPa

H12

EN 573-3

Wire, Flat, Seamless Tube

300.0 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

H12

EN 573-3

Wire, Flat, Seamless Tube

Elongation

4.0 %

Show Material materials with Elongation of 4.0 %

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A50

5.0 %

Show Material materials with Elongation of 5.0 %

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A50

6.0 %

Show Material materials with Elongation of 6.0 %

H12

EN 573-3, EN 1301

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

6.0 %

Show Material materials with Elongation of 6.0 %

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A50

7.0 %

Show Material materials with Elongation of 7.0 %

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A50

9.0 %

Show Material materials with Elongation of 9.0 %

H12

EN 573-3, EN 1592, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A100

9.0 %

Show Material materials with Elongation of 9.0 %

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A50

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

H12

EN 573-3

Flat

A50 Transverse

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

H12

EN 573-3

Flat

A50

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H12

EN 573-3

Flat

A50 Transverse

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H12

EN 573-3

Flat

A50

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

H12

EN 573-3

Wire

A100

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

H12

EN 573-3

Flat

A50 Transverse

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

H12

EN 573-3

Flat

A50

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

H12

EN 573-3

Flat

A50 Transverse

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

H12

EN 573-3

Flat

A50

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

H12

EN 573-3

Flat

A50 Transverse

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

H12

EN 573-3

Flat

Transverse

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

H12

EN 573-3

Seamless Tube, Flat

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

H12

EN 573-3

Flat

A50

Hardness, Brinell

66.0 [-]

Show Material materials with Hardness, Brinell of 66.0 [-]

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

20.0 °C

66.0 [-]

Show Material materials with Hardness, Brinell of 66.0 [-]

H12

EN 573-3

Flat

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

H12

EN 573-3

Wire, Flat, Seamless Tube

Shear modulus

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

H12

EN 573-3, EN 1301, EN 1592, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

20.0 °C

26.5 - 27.0 GPa

Show Material materials with Shear modulus of 26.5 - 27.0 GPa

H12

EN 573-3

Wire, Flat, Seamless Tube

20.0 °C

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

H12

EN 573-3

Wire, Flat, Seamless Tube

Tensile strength

220.0 MPa

Show Material materials with Tensile strength of 220.0 MPa

H12

EN 573-3, EN 1592

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

20.0 °C

220.0 MPa

Show Material materials with Tensile strength of 220.0 MPa

H12

EN 573-3

Seamless Tube

20.0 °C

220.0 - 270.0 MPa

Show Material materials with Tensile strength of 220.0 - 270.0 MPa

H12

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Wire, Forging, Tube, Bar

20.0 °C

220.0 - 270.0 MPa

Show Material materials with Tensile strength of 220.0 - 270.0 MPa

H12

EN 573-3

Flat

Transverse

20.0 °C

230.0 - 280.0 MPa

Show Material materials with Tensile strength of 230.0 - 280.0 MPa

H12

EN 573-3, EN 1301

Wire, Strip, Sheet, Plate, Forging, Tube, Bar

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.3899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3899999999999998e-05 1/K

H12

EN 573-3, EN 1301, EN 1592, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

100 °C

2.3899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3899999999999998e-05 1/K

H12

EN 573-3, EN 1301, EN 1592, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

100.0 °C

2.39e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.39e-05 1/K

H12

EN 573-3

Wire, Flat, Seamless Tube

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

610.0 - 640.0 °C

Show Material materials with Melting point of 610.0 - 640.0 °C

H12

EN 573-3, EN 1301, EN 1592, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

Specific heat capacity

20.0 °C

897.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 897.0 - 963.0 J/(kg·K)

H12

EN 573-3

Wire, Flat, Seamless Tube

20.0 °C

897.0 J/(kg·K)

Show Material materials with Specific heat capacity of 897.0 J/(kg·K)

H12

EN 573-3

Wire, Flat, Seamless Tube

20.0 °C

963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 963.0 J/(kg·K)

H12

EN 573-3

Wire, Flat, Seamless Tube

Thermal conductivity

20.0 °C

132.0 - 160.0 W/(m·K)

Show Material materials with Thermal conductivity of 132.0 - 160.0 W/(m·K)

H12

EN 573-3

Wire, Flat, Seamless Tube

20.0 °C

132.0 - 140.0 W/(m·K)

Show Material materials with Thermal conductivity of 132.0 - 140.0 W/(m·K)

H12

EN 573-3

Wire, Flat, Seamless Tube

20.0 °C

132.0 W/(m·K)

Show Material materials with Thermal conductivity of 132.0 W/(m·K)

H12

EN 573-3

Wire, Flat, Seamless Tube

20.0 °C

140.0 - 160.0 W/(m·K)

Show Material materials with Thermal conductivity of 140.0 - 160.0 W/(m·K)

H12

EN 573-3, EN 1301, EN 1592, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Flat, Seamless Tube

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

20000000.0 - 23000000.0 S/m

Show Material materials with Electrical conductivity of 20000000.0 - 23000000.0 S/m

H12

EN 573-3, EN 1301, EN 1592, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Flat, Seamless Tube

Electrical resistivity

4.35e-08 - 5e-08 Ω·m

Show Material materials with Electrical resistivity of 4.35e-08 - 5e-08 Ω·m

H12

EN 573-3, EN 1301, EN 1592, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

20.0 °C

4.3e-08 - 5.3e-08 Ω·m

Show Material materials with Electrical resistivity of 4.3e-08 - 5.3e-08 Ω·m

H12

EN 573-3

Wire, Flat, Seamless Tube

20.0 °C

4.3e-08 - 5e-08 Ω·m

Show Material materials with Electrical resistivity of 4.3e-08 - 5e-08 Ω·m

H12

EN 573-3

Wire, Flat, Seamless Tube

20.0 °C

5e-08 - 5.3e-08 Ω·m

Show Material materials with Electrical resistivity of 5e-08 - 5.3e-08 Ω·m

H12

EN 573-3

Wire, Flat, Seamless Tube

20.0 °C

5.3e-08 Ω·m

Show Material materials with Electrical resistivity of 5.3e-08 Ω·m

H12

EN 573-3

Wire, Flat, Seamless Tube

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.3 %

Show Material materials with Chromium of 0.3 %

H12

EN 573-3, EN 1301, EN 1592, EN 485

Wire, Flat, Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Bar

Copper

0.1 %

Show Material materials with Copper of 0.1 %

H12

EN 573-3, EN 1301, EN 1592, EN 485

Wire, Flat, Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Bar

Iron

0.4 %

Show Material materials with Iron of 0.4 %

H12

EN 573-3

Wire, Flat, Seamless Tube

0.40 %

Show Material materials with Iron of 0.40 %

H12

EN 573-3, EN 1301, EN 1592, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

Magnesium

2.6 - 3.6 %

Show Material materials with Magnesium of 2.6 - 3.6 %

H12

EN 573-3, EN 1301, EN 1592, EN 485

Wire, Flat, Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Bar

Manganese

0.5 %

Show Material materials with Manganese of 0.5 %

H12

EN 573-3, EN 1301, EN 1592, EN 485

Wire, Flat, Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Bar

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

H12

EN 573-3, EN 1301, EN 1592, EN 485

Wire, Flat, Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Bar

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

H12

EN 573-3, EN 1301, EN 1592, EN 485

Wire, Flat, Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Bar

Zinc

0.2 %

Show Material materials with Zinc of 0.2 %

H12

EN 573-3, EN 1301, EN 1592, EN 485

Wire, Flat, Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Bar

Technological properties

Property
Anodizing

decorative: gut (EQ: sehr gut), Protective: very good

Brazing

hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor

Corrosion properties

Seawater: very good to good, weathering: very good

Workability