EN 573-3 Grade AW-5754 H32

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlMg alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey,Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.66 g/cm³

Show Material materials with Density of 2.66 g/cm³

H32

EN 573-3, EN 1301, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

2.67 g/cm³

Show Material materials with Density of 2.67 g/cm³

H32

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

20.0 °C

2.66 g/cm³

Show Material materials with Density of 2.66 g/cm³

H32

EN 573-3

Wire, Flat

20.0 °C

2.66 - 2.68 g/cm³

Show Material materials with Density of 2.66 - 2.68 g/cm³

H32

EN 573-3

Wire, Flat

20.0 °C

2.68 g/cm³

Show Material materials with Density of 2.68 g/cm³

H32

EN 573-3

Wire, Flat

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

1.5 mm

Show Material materials with Thickness of 1.5 mm

H32

EN 573-1, EN 573-2, EN 573-3, EN 485-2

1.5 mm

Sheet, Strip, Plate

3.0 mm

Show Material materials with Thickness of 3.0 mm

H32

EN 573-1, EN 573-2, EN 573-3, EN 485-2

3.0 mm

Sheet, Strip, Plate

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending angle 180°

1.5 °/t

Show Material materials with Bending angle 180° of 1.5 °/t

H32

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

2.0 °/t

Show Material materials with Bending angle 180° of 2.0 °/t

H32

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

2 °/t

Show Material materials with Bending angle 180° of 2 °/t

H32

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

Bending angle 90°

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

H32

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

H32

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

1.5 °/t

Show Material materials with Bending angle 90° of 1.5 °/t

H32

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

1.5 °/t

Show Material materials with Bending angle 90° of 1.5 °/t

H32

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

2.5 °/t

Show Material materials with Bending angle 90° of 2.5 °/t

H32

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

Elastic modulus

-270.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H32

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3

Sheet, Strip, Plate, Wire, Flat

70.5 GPa

Show Material materials with Elastic modulus of 70.5 GPa

H32

EN 573-3, EN 1301, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H32

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3

Sheet, Strip, Plate, Wire, Flat

20.0 °C

70.0 - 70.5 GPa

Show Material materials with Elastic modulus of 70.0 - 70.5 GPa

H32

EN 573-3

Wire, Flat

20.0 °C

70.5 GPa

Show Material materials with Elastic modulus of 70.5 GPa

H32

EN 573-3

Wire, Flat

50.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H32

EN 573-3

Wire, Flat

100.0 °C

68.0 GPa

Show Material materials with Elastic modulus of 68.0 GPa

H32

EN 573-3

Wire, Flat

150.0 °C

66.0 GPa

Show Material materials with Elastic modulus of 66.0 GPa

H32

EN 573-3

Wire, Flat

200.0 °C

63.0 GPa

Show Material materials with Elastic modulus of 63.0 GPa

H32

EN 573-3

Wire, Flat

250.0 °C

57.0 GPa

Show Material materials with Elastic modulus of 57.0 GPa

H32

EN 573-3

Wire, Flat

300.0 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

H32

EN 573-3

Wire, Flat

Elongation

7.0 %

Show Material materials with Elongation of 7.0 %

H32

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A50

7.0 - 11.0 %

Show Material materials with Elongation of 7.0 - 11.0 %

H32

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

A50

8.0 %

Show Material materials with Elongation of 8.0 %

H32

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A50

9.0 %

Show Material materials with Elongation of 9.0 %

H32

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A100

10.0 %

Show Material materials with Elongation of 10.0 %

H32

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A50

11.0 %

Show Material materials with Elongation of 11.0 %

H32

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A50

11.0 %

Show Material materials with Elongation of 11.0 %

H32

EN 573-3, EN 1301

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

H32

EN 573-3

Flat

A50 Transverse

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

H32

EN 573-3

Flat

A50

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

H32

EN 573-3

Flat

A50 Transverse

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

H32

EN 573-3

Flat

A50

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

H32

EN 573-3

Flat

Transverse

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

H32

EN 573-3

Flat

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

H32

EN 573-3

Flat

A50 Transverse

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

H32

EN 573-3

Flat

A50

20.0 °C

11.0 %

Show Material materials with Elongation of 11.0 %

H32

EN 573-3

Wire

A100

20.0 °C

11.0 %

Show Material materials with Elongation of 11.0 %

H32

EN 573-3

Flat

A50 Transverse

20.0 °C

11.0 %

Show Material materials with Elongation of 11.0 %

H32

EN 573-3

Flat

A50

Hardness, Brinell

63.0 [-]

Show Material materials with Hardness, Brinell of 63.0 [-]

H32

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

20.0 °C

63.0 [-]

Show Material materials with Hardness, Brinell of 63.0 [-]

H32

EN 573-3

Flat

Hardness, HBW

63 [-]

Show Material materials with Hardness, HBW of 63 [-]

H32

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

H32

EN 573-3

Wire, Flat

Shear modulus

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

H32

EN 573-3, EN 1301, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

27.0 GPa

Show Material materials with Shear modulus of 27.0 GPa

H32

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

20.0 °C

26.5 - 27.0 GPa

Show Material materials with Shear modulus of 26.5 - 27.0 GPa

H32

EN 573-3

Wire, Flat

20.0 °C

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

H32

EN 573-3

Wire, Flat

Tensile strength

20.0 °C

220.0 - 270.0 MPa

Show Material materials with Tensile strength of 220.0 - 270.0 MPa

H32

EN 573-3, EN 1301, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Wire, Flat, Strip, Sheet, Plate, Forging, Tube, Bar, Strip, Plate

20.0 °C

220.0 - 270.0 MPa

Show Material materials with Tensile strength of 220.0 - 270.0 MPa

H32

EN 573-3

Flat

Transverse

Yield strength

130.0 MPa

Show Material materials with Yield strength of 130.0 MPa

H32

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

RP02

130 MPa

Show Material materials with Yield strength of 130 MPa

H32

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

160.0 MPa

Show Material materials with Yield strength of 160.0 MPa

H32

EN 573-3, EN 1301

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

RP02

20.0 °C

130.0 MPa

Show Material materials with Yield strength of 130.0 MPa

H32

EN 573-3

Flat

RP02

20.0 °C

130.0 MPa

Show Material materials with Yield strength of 130.0 MPa

H32

EN 573-3

Flat

RP02 Transverse

20.0 °C

160.0 MPa

Show Material materials with Yield strength of 160.0 MPa

H32

EN 573-3

Wire

RP02

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.3899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3899999999999998e-05 1/K

H32

EN 573-3, EN 1301, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

100 °C

2.3899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3899999999999998e-05 1/K

H32

EN 573-3, EN 1301, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

100.0 °C

2.39e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.39e-05 1/K

H32

EN 573-3

Wire, Flat

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

H32

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

20-100°C

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

610.0 - 640.0 °C

Show Material materials with Melting point of 610.0 - 640.0 °C

H32

EN 573-3, EN 1301, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

Specific heat capacity

20.0 °C

897.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 897.0 - 963.0 J/(kg·K)

H32

EN 573-3

Wire, Flat

20.0 °C

897.0 J/(kg·K)

Show Material materials with Specific heat capacity of 897.0 J/(kg·K)

H32

EN 573-3

Wire, Flat

20.0 °C

963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 963.0 J/(kg·K)

H32

EN 573-3

Wire, Flat

Thermal conductivity

147.0 - 168.0 W/(m·K)

Show Material materials with Thermal conductivity of 147.0 - 168.0 W/(m·K)

H32

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

20.0 °C

132.0 - 160.0 W/(m·K)

Show Material materials with Thermal conductivity of 132.0 - 160.0 W/(m·K)

H32

EN 573-3

Wire, Flat

20.0 °C

132.0 - 140.0 W/(m·K)

Show Material materials with Thermal conductivity of 132.0 - 140.0 W/(m·K)

H32

EN 573-3

Wire, Flat

20.0 °C

132.0 W/(m·K)

Show Material materials with Thermal conductivity of 132.0 W/(m·K)

H32

EN 573-3

Wire, Flat

20.0 °C

140.0 - 160.0 W/(m·K)

Show Material materials with Thermal conductivity of 140.0 - 160.0 W/(m·K)

H32

EN 573-3, EN 1301, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Flat

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

20000000.0 - 23000000.0 S/m

Show Material materials with Electrical conductivity of 20000000.0 - 23000000.0 S/m

H32

EN 573-3, EN 1301, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Flat

Electrical resistivity

4.35e-08 - 5e-08 Ω·m

Show Material materials with Electrical resistivity of 4.35e-08 - 5e-08 Ω·m

H32

EN 573-3, EN 1301, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

4.9e-08 Ω·m

Show Material materials with Electrical resistivity of 4.9e-08 Ω·m

H32

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

20.0 °C

4.3e-08 - 5.3e-08 Ω·m

Show Material materials with Electrical resistivity of 4.3e-08 - 5.3e-08 Ω·m

H32

EN 573-3

Wire, Flat

20.0 °C

4.3e-08 - 5e-08 Ω·m

Show Material materials with Electrical resistivity of 4.3e-08 - 5e-08 Ω·m

H32

EN 573-3

Wire, Flat

20.0 °C

5e-08 - 5.3e-08 Ω·m

Show Material materials with Electrical resistivity of 5e-08 - 5.3e-08 Ω·m

H32

EN 573-3

Wire, Flat

20.0 °C

5.3e-08 Ω·m

Show Material materials with Electrical resistivity of 5.3e-08 Ω·m

H32

EN 573-3

Wire, Flat

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.3 %

Show Material materials with Chromium of 0.3 %

H32

EN 573-3, EN 1301, EN 485

Wire, Flat, Strip, Sheet, Plate, Forging, Tube, Bar

0.3 %

Show Material materials with Chromium of 0.3 %

H32

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

Copper

0.1 %

Show Material materials with Copper of 0.1 %

H32

EN 573-3, EN 1301, EN 485

Wire, Flat, Strip, Sheet, Plate, Forging, Tube, Bar

0.1 %

Show Material materials with Copper of 0.1 %

H32

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

Iron

0.4 %

Show Material materials with Iron of 0.4 %

H32

EN 573-3

Wire, Flat

0.40 %

Show Material materials with Iron of 0.40 %

H32

EN 573-3, EN 1301, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

0.4 %

Show Material materials with Iron of 0.4 %

H32

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

Magnesium

2.6 - 3.6 %

Show Material materials with Magnesium of 2.6 - 3.6 %

H32

EN 573-3, EN 1301, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Wire, Flat, Strip, Sheet, Plate, Forging, Tube, Bar, Strip, Plate

Manganese

0.5 %

Show Material materials with Manganese of 0.5 %

H32

EN 573-3, EN 1301, EN 485

Wire, Flat, Strip, Sheet, Plate, Forging, Tube, Bar

0.5 %

Show Material materials with Manganese of 0.5 %

H32

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

Other

0.1 - 0.6 %

Show Material materials with Other of 0.1 - 0.6 %

H32

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

H32

EN 573-3, EN 1301, EN 485

Wire, Flat, Strip, Sheet, Plate, Forging, Tube, Bar

0.4 %

Show Material materials with Silicon of 0.4 %

H32

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

H32

EN 573-3, EN 1301, EN 485

Wire, Flat, Strip, Sheet, Plate, Forging, Tube, Bar

0.15 %

Show Material materials with Titanium of 0.15 %

H32

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

Zinc

0.2 %

Show Material materials with Zinc of 0.2 %

H32

EN 573-3, EN 1301, EN 485

Wire, Flat, Strip, Sheet, Plate, Forging, Tube, Bar

0.2 %

Show Material materials with Zinc of 0.2 %

H32

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Plate

Technological properties

Property
Anodizing

decorative: gut (EQ: sehr gut), Protective: very good

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Electronic devices: Housing of devices; Tubes: Industrial tubes, Pipes; Wind energy: Nacelle coverings, rotor hub, stairs; Components: Heat shields, Access hatches, Spoilers, Fuel and oil tanks, General transportation

Brazing

hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor

Corrosion properties

Seawater: very good to good, weathering: very good

Welding

Very Good

Workability

Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12)