General
Property | Value | Comment |
---|---|---|
Density | 2.7 g/cm³ Show Material materials with Density of 2.7 g/cm³ | Typical for Wrought 6000 Series Aluminium |
Mechanical
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Elastic modulus | 70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | Typical for Wrought 6000 Series Aluminium | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||
Shear modulus | 26.0 - 26.5 GPa Show Material materials with Shear modulus of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | ||
Tensile strength | 260.0 MPa Show Material materials with Tensile strength of 260.0 MPa | T6 | AA Standards, ASTM B221 | |
290.0 MPa Show Material materials with Tensile strength of 290.0 MPa | T6 | AA Standards, ASTM B210, ASTM B211, ASTM B483 |
Thermal
Property | Value | Comment |
---|---|---|
Coefficient of thermal expansion | 1.6e-05 - 2.4e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.6e-05 - 2.4e-05 1/K | Typical for Wrought 6000 Series Aluminium |
Melting point | 555.0 - 655.0 °C Show Material materials with Melting point of 555.0 - 655.0 °C | Typical for Wrought 6000 Series Aluminium |
Specific heat capacity | 887.0 - 963.0 J/(kg·K) Show Material materials with Specific heat capacity of 887.0 - 963.0 J/(kg·K) | Typical for Wrought 6000 Series Aluminium |
Thermal conductivity | 170.0 - 220.0 W/(m·K) Show Material materials with Thermal conductivity of 170.0 - 220.0 W/(m·K) | Typical for Wrought 6000 Series Aluminium |
Electrical
Property | Value | Comment |
---|---|---|
Electrical conductivity | 21000000.0 - 34000000.0 S/m Show Material materials with Electrical conductivity of 21000000.0 - 34000000.0 S/m | Typical for Wrought 6000 Series Aluminium |
Electrical resistivity | 2.9e-08 - 5e-08 Ω·m Show Material materials with Electrical resistivity of 2.9e-08 - 5e-08 Ω·m | Typical for Wrought 6000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Bismuth | 0.4 - 0.7 % Show Material materials with Bismuth of 0.4 - 0.7 % | T6 | AA Standards, ASTM B210, ASTM B211, ASTM B221, ASTM B483 |
Chromium | 0.04 - 0.14 % Show Material materials with Chromium of 0.04 - 0.14 % | T6 | AA Standards, ASTM B210, ASTM B211, ASTM B221, ASTM B483 |
Copper | 0.15 - 0.4 % Show Material materials with Copper of 0.15 - 0.4 % | T6 | AA Standards, ASTM B210, ASTM B211, ASTM B221, ASTM B483 |
Iron | 0.70 % Show Material materials with Iron of 0.70 % | T6 | AA Standards, ASTM B210, ASTM B211, ASTM B221, ASTM B483 |
Lead | 0.4 - 0.7 % Show Material materials with Lead of 0.4 - 0.7 % | T6 | AA Standards, ASTM B210, ASTM B211, ASTM B221, ASTM B483 |
Magnesium | 0.8 - 1.2 % Show Material materials with Magnesium of 0.8 - 1.2 % | T6 | AA Standards, ASTM B210, ASTM B211, ASTM B221, ASTM B483 |
Manganese | 0.15 % Show Material materials with Manganese of 0.15 % | T6 | AA Standards, ASTM B210, ASTM B211, ASTM B221, ASTM B483 |
Silicon | 0.4 - 0.8 % Show Material materials with Silicon of 0.4 - 0.8 % | T6 | AA Standards, ASTM B210, ASTM B211, ASTM B221, ASTM B483 |
Titanium | 0.15 % Show Material materials with Titanium of 0.15 % | T6 | AA Standards, ASTM B210, ASTM B211, ASTM B221, ASTM B483 |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | T6 | AA Standards, ASTM B210, ASTM B211, ASTM B221, ASTM B483 |
Technological properties
Property | ||
---|---|---|
Brazing | general: Lötbar mit speziellen Techniken oder bei bestimmten Anwendungen | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: good, without protection in industrial or seawater atmosphere | |
General machinability | General: good to acceptable (T6, T651, T6510, T6511, T9) | |
Workability | general (condition): poor(T6, T651, T6510, T6511), not suitable (T9) |