AA Standards Grade 6005 T5

Want to keep this datasheet? Save it now in your required format

Related Standards

Equivalent Materials

This material data has been provided by AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated Standards

Density

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

T5

AA Standards, ASTM B221

Mechanical

PropertyValueConditionRelated StandardsComment

Elastic modulus

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

Typical for Wrought 6000 Series Aluminium

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 6000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 6000 Series Aluminium

Shear modulus

26.0 - 26.5 GPa

Show Material materials with Shear modulus of 26.0 - 26.5 GPa

Typical for Wrought 6000 Series Aluminium

Tensile strength

260.0 MPa

Show Material materials with Tensile strength of 260.0 MPa

T5

AA Standards, ASTM B221

Thermal

PropertyTemperatureValueConditionRelated StandardsComment

Coefficient of thermal expansion

100 °C, 20 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

T5

AA Standards, ASTM B221

Melting point

605.0 - 655.0 °C

Show Material materials with Melting point of 605.0 - 655.0 °C

T5

AA Standards, ASTM B221

Specific heat capacity

887.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 887.0 - 963.0 J/(kg·K)

Typical for Wrought 6000 Series Aluminium

Thermal conductivity

180.0 - 188.0 W/(m·K)

Show Material materials with Thermal conductivity of 180.0 - 188.0 W/(m·K)

T5

AA Standards, ASTM B221

Electrical

PropertyValueConditionRelated Standards

Electrical conductivity

27000000.0 - 28000000.0 S/m

Show Material materials with Electrical conductivity of 27000000.0 - 28000000.0 S/m

T5

AA Standards, ASTM B221

Electrical resistivity

3.57e-08 - 3.7e-08 Ω·m

Show Material materials with Electrical resistivity of 3.57e-08 - 3.7e-08 Ω·m

T5

AA Standards, ASTM B221

Chemical properties

PropertyValueConditionRelated Standards

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

T5

AA Standards, ASTM B221

Copper

0.1 %

Show Material materials with Copper of 0.1 %

T5

AA Standards, ASTM B221

Iron

0.35 %

Show Material materials with Iron of 0.35 %

T5

AA Standards, ASTM B221

Magnesium

0.4 - 0.6 %

Show Material materials with Magnesium of 0.4 - 0.6 %

T5

AA Standards, ASTM B221

Manganese

0.1 %

Show Material materials with Manganese of 0.1 %

T5

AA Standards, ASTM B221

Silicon

0.6 - 0.9 %

Show Material materials with Silicon of 0.6 - 0.9 %

T5

AA Standards, ASTM B221

Titanium

0.1 %

Show Material materials with Titanium of 0.1 %

T5

AA Standards, ASTM B221

Zinc

0.1 %

Show Material materials with Zinc of 0.1 %

T5

AA Standards, ASTM B221

Technological properties

Property
Brazing

general: possible with commercial processes and methods

Workability

Excellent workability.