EN 573-3 Grade AW-6060 H19

Want to keep this datasheet? Save it now in your required format

Description

Age-hardenable AlMgSi alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H19

EN 573-3, EN 683

Strip, Sheet, Plate, Tube, Bar

20.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H19

EN 573-3

Foil

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

H19

EN 573-3, EN 683

Strip, Sheet, Plate, Tube, Bar

20.0 °C

67.0 GPa

Show Material materials with Elastic modulus of 67.0 GPa

H19

EN 573-3

Foil

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 6000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 6000 Series Aluminium

Shear modulus

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

H19

EN 573-3, EN 683

Strip, Sheet, Plate, Tube, Bar

20.0 °C

25.0 GPa

Show Material materials with Shear modulus of 25.0 GPa

H19

EN 573-3

Foil

Tensile strength

200.0 MPa

Show Material materials with Tensile strength of 200.0 MPa

H19

EN 573-3, EN 683

Strip, Sheet, Plate, Tube, Bar

20.0 °C

200.0 MPa

Show Material materials with Tensile strength of 200.0 MPa

H19

EN 573-3

Foil

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

-50 °C

2.18e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.18e-05 1/K

H19

EN 573-3, EN 683

Strip, Sheet, Plate, Tube, Bar

20 °C

2.18e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.18e-05 1/K

H19

EN 573-3, EN 683

Strip, Sheet, Plate, Tube, Bar

20 °C

2.3399999999999996e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K

H19

EN 573-3, EN 683

Strip, Sheet, Plate, Tube, Bar

20 °C

2.45e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.45e-05 1/K

H19

EN 573-3, EN 683

Strip, Sheet, Plate, Tube, Bar

20 °C

2.56e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.56e-05 1/K

H19

EN 573-3, EN 683

Strip, Sheet, Plate, Tube, Bar

100 °C

2.3399999999999996e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K

H19

EN 573-3, EN 683

Strip, Sheet, Plate, Tube, Bar

200 °C

2.45e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.45e-05 1/K

H19

EN 573-3, EN 683

Strip, Sheet, Plate, Tube, Bar

300 °C

2.56e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.56e-05 1/K

H19

EN 573-3, EN 683

Strip, Sheet, Plate, Tube, Bar

Melting point

585.0 - 650.0 °C

Show Material materials with Melting point of 585.0 - 650.0 °C

H19

EN 573-3, EN 683

Strip, Sheet, Plate, Tube, Bar

Specific heat capacity

898.0 J/(kg·K)

Show Material materials with Specific heat capacity of 898.0 J/(kg·K)

H19

EN 573-3, EN 683

Strip, Sheet, Plate, Tube, Bar

Thermal conductivity

200.0 - 220.0 W/(m·K)

Show Material materials with Thermal conductivity of 200.0 - 220.0 W/(m·K)

H19

EN 573-3, EN 683

Strip, Sheet, Plate, Tube, Bar

20.0 °C

220.0 W/(m·K)

Show Material materials with Thermal conductivity of 220.0 W/(m·K)

H19

EN 573-3

Foil

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

28000000.0 - 31000000.0 S/m

Show Material materials with Electrical conductivity of 28000000.0 - 31000000.0 S/m

H19

EN 573-3, EN 683

Strip, Sheet, Plate, Tube, Bar

20.0 °C

30000000.0 - 32000000.0 S/m

Show Material materials with Electrical conductivity of 30000000.0 - 32000000.0 S/m

H19

EN 573-3

Foil

Electrical resistivity

3.23e-08 - 3.57e-08 Ω·m

Show Material materials with Electrical resistivity of 3.23e-08 - 3.57e-08 Ω·m

H19

EN 573-3, EN 683

Strip, Sheet, Plate, Tube, Bar

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.05 %

Show Material materials with Chromium of 0.05 %

H19

EN 573-3, EN 683

Foil, Strip, Sheet, Plate, Tube, Bar

Copper

0.1 %

Show Material materials with Copper of 0.1 %

H19

EN 573-3, EN 683

Foil, Strip, Sheet, Plate, Tube, Bar

Iron

0.1 - 0.3 %

Show Material materials with Iron of 0.1 - 0.3 %

H19

EN 573-3, EN 683

Foil, Strip, Sheet, Plate, Tube, Bar

Magnesium

0.35 - 0.6 %

Show Material materials with Magnesium of 0.35 - 0.6 %

H19

EN 573-3, EN 683

Foil, Strip, Sheet, Plate, Tube, Bar

Manganese

0.1 %

Show Material materials with Manganese of 0.1 %

H19

EN 573-3, EN 683

Foil, Strip, Sheet, Plate, Tube, Bar

Silicon

0.3 - 0.6 %

Show Material materials with Silicon of 0.3 - 0.6 %

H19

EN 573-3, EN 683

Foil, Strip, Sheet, Plate, Tube, Bar

Titanium

0.1 %

Show Material materials with Titanium of 0.1 %

H19

EN 573-3, EN 683

Foil, Strip, Sheet, Plate, Tube, Bar

Zinc

0.15 %

Show Material materials with Zinc of 0.15 %

H19

EN 573-3, EN 683

Foil, Strip, Sheet, Plate, Tube, Bar

Technological properties

Property
Anodizing

decorative: EQ: sehr gut, Protective: very good

Brazing

hard brazing (with flux/ without flux): very good / good, friction soldering: very good, soft brazing with flux: good

Corrosion properties

Seawater: good, weathering: very good

Workability

Bending / Spinning (cold): acceptable (T3, T4) / -, Impact extrusion (cold): good (O), Deep drawing / upsetting (Condition) - / good (O)