EN 573-3 Grade AW-6060 T4

Want to keep this datasheet? Save it now in your required format

Description

Age-hardenable AlMgSi alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar

20.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

T4

EN 573-3

Profile, Rod, Tube, Wire

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

-270 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

T4

EN 573-3

Strip, Sheet, Plate, Tube, Bar

-196.0 °C

65.0 GPa

Show Material materials with Elastic modulus of 65.0 GPa

T4

EN 573-3

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

T4

EN 573-3

Strip, Sheet, Plate, Tube, Bar

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar

20.0 °C

65.0 GPa

Show Material materials with Elastic modulus of 65.0 GPa

T4

EN 573-3

20.0 °C

67.0 GPa

Show Material materials with Elastic modulus of 67.0 GPa

T4

EN 573-3

Profile, Rod, Tube, Wire

20 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

T4

EN 573-3

Strip, Sheet, Plate, Tube, Bar

50.0 °C

65.0 GPa

Show Material materials with Elastic modulus of 65.0 GPa

T4

EN 573-3

300 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

T4

EN 573-3

Strip, Sheet, Plate, Tube, Bar

Elongation

10.0 %

Show Material materials with Elongation of 10.0 %

T4

EN 573-3, EN 754

Strip, Sheet, Plate, Tube, Bar

A50

12.0 %

Show Material materials with Elongation of 12.0 %

T4

EN 573-3, EN 754

Strip, Sheet, Plate, Tube, Bar

A100

13.0 %

Show Material materials with Elongation of 13.0 %

T4

EN 573-3, EN 754

Strip, Sheet, Plate, Tube, Bar

A50

13.0 %

Show Material materials with Elongation of 13.0 %

T4

EN 573-3, EN 1301

Strip, Sheet, Plate, Tube, Bar

14.0 %

Show Material materials with Elongation of 14.0 %

T4

EN 573-3, EN 12020, EN 755

Strip, Sheet, Plate, Tube, Bar

A50

15.0 %

Show Material materials with Elongation of 15.0 %

T4

EN 573-3

Strip, Sheet, Plate, Tube, Bar

15.0 %

Show Material materials with Elongation of 15.0 %

T4

EN 573-3, EN 754

Strip, Sheet, Plate, Tube, Bar

A100

16.0 %

Show Material materials with Elongation of 16.0 %

T4

EN 573-3, EN 12020, EN 755

Strip, Sheet, Plate, Tube, Bar

A100

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

T4

EN 573-3

Tube

A50

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

T4

EN 573-3

Tube

20.0 °C

13.0 %

Show Material materials with Elongation of 13.0 %

T4

EN 573-3

Rod, Tube

A50

20.0 °C

13.0 %

Show Material materials with Elongation of 13.0 %

T4

EN 573-3

Wire

A100

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

T4

EN 573-3

Profile, Rod, Tube

A50

20.0 °C

15.0 %

Show Material materials with Elongation of 15.0 %

T4

EN 573-3

Rod, Tube, Profile

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

T4

EN 573-3

Rod, Tube, Profile

Hardness, Brinell

20.0 °C

50.0 [-]

Show Material materials with Hardness, Brinell of 50.0 [-]

T4

EN 573-3

Profile, Rod, Tube

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 6000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 6000 Series Aluminium

Shear modulus

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar

20.0 °C

25.0 GPa

Show Material materials with Shear modulus of 25.0 GPa

T4

EN 573-3

Profile, Rod, Tube, Wire

Tensile strength

120.0 MPa

Show Material materials with Tensile strength of 120.0 MPa

T4

EN 573-3, EN 12020, EN 755

Strip, Sheet, Plate, Tube, Bar

130.0 MPa

Show Material materials with Tensile strength of 130.0 MPa

T4

EN 573-3, EN 754

Strip, Sheet, Plate, Tube, Bar

140.0 MPa

Show Material materials with Tensile strength of 140.0 MPa

T4

EN 573-3, EN 1301

Strip, Sheet, Plate, Tube, Bar

155.0 - 210.0 MPa

Show Material materials with Tensile strength of 155.0 - 210.0 MPa

T4

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Tube, Bar

20.0 °C

120.0 MPa

Show Material materials with Tensile strength of 120.0 MPa

T4

EN 573-3

Rod, Tube, Profile

20.0 °C

130.0 MPa

Show Material materials with Tensile strength of 130.0 MPa

T4

EN 573-3

Rod, Tube, Profile

20.0 °C

140.0 - 210.0 MPa

Show Material materials with Tensile strength of 140.0 - 210.0 MPa

T4

EN 573-3

Wire

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

-50 °C

2.18e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.18e-05 1/K

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar

20 °C

2.18e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.18e-05 1/K

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar

20 °C

2.3399999999999996e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar

20 °C

2.45e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.45e-05 1/K

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar

20 °C

2.56e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.56e-05 1/K

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar

100 °C

2.3399999999999996e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar

200 °C

2.45e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.45e-05 1/K

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar

300 °C

2.56e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.56e-05 1/K

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar

Melting point

585.0 - 650.0 °C

Show Material materials with Melting point of 585.0 - 650.0 °C

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar

Specific heat capacity

898.0 J/(kg·K)

Show Material materials with Specific heat capacity of 898.0 J/(kg·K)

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar

Thermal conductivity

200.0 - 220.0 W/(m·K)

Show Material materials with Thermal conductivity of 200.0 - 220.0 W/(m·K)

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar

20.0 °C

220.0 W/(m·K)

Show Material materials with Thermal conductivity of 220.0 W/(m·K)

T4

EN 573-3

Profile, Rod, Tube, Wire

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

28000000.0 - 31000000.0 S/m

Show Material materials with Electrical conductivity of 28000000.0 - 31000000.0 S/m

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar

20.0 °C

30000000.0 - 32000000.0 S/m

Show Material materials with Electrical conductivity of 30000000.0 - 32000000.0 S/m

T4

EN 573-3

Profile, Rod, Tube, Wire

Electrical resistivity

3.23e-08 - 3.57e-08 Ω·m

Show Material materials with Electrical resistivity of 3.23e-08 - 3.57e-08 Ω·m

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.05 %

Show Material materials with Chromium of 0.05 %

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Profile, Rod, Tube, Wire, Strip, Sheet, Plate, Bar

Copper

0.1 %

Show Material materials with Copper of 0.1 %

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Profile, Rod, Tube, Wire, Strip, Sheet, Plate, Bar

Iron

0.1 - 0.3 %

Show Material materials with Iron of 0.1 - 0.3 %

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Profile, Rod, Tube, Wire, Strip, Sheet, Plate, Bar

Magnesium

0.35 - 0.6 %

Show Material materials with Magnesium of 0.35 - 0.6 %

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Profile, Rod, Tube, Wire, Strip, Sheet, Plate, Bar

Manganese

0.1 %

Show Material materials with Manganese of 0.1 %

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Profile, Rod, Tube, Wire, Strip, Sheet, Plate, Bar

Silicon

0.3 - 0.6 %

Show Material materials with Silicon of 0.3 - 0.6 %

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Profile, Rod, Tube, Wire, Strip, Sheet, Plate, Bar

Titanium

0.1 %

Show Material materials with Titanium of 0.1 %

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Profile, Rod, Tube, Wire, Strip, Sheet, Plate, Bar

Zinc

0.15 %

Show Material materials with Zinc of 0.15 %

T4

EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755

Profile, Rod, Tube, Wire, Strip, Sheet, Plate, Bar

Technological properties

Property
Anodizing

decorative: EQ: sehr gut, Protective: very good

Brazing

hard brazing (with flux/ without flux): very good / good, friction soldering: very good, soft brazing with flux: good

Corrosion properties

Seawater: good, weathering: very good

Workability