EN 573-3 Grade AW-6063 F

Want to keep this datasheet? Save it now in your required format

Description

Aluminum EN AW-6063 is an architectural alloy that offers users a high resistance to corrosion and excellent finishing characteristics. Easy to extrude with fair machinability, EN AW-6063 can be both hot and cold formed and is commonly available as T6 temper as well as T4 temper.

Related Standards

Equivalent Materials

This material data has been provided by AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated StandardsShape

Density

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

F

EN 573-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Mechanical

PropertyValueConditionRelated StandardsShapeComment

Elastic modulus

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

F

EN 573-3, EN 570

Strip, Sheet, Plate, Tube, Bar

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

F

EN 573-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Hardness, Brinell

37.0 [-]

Show Material materials with Hardness, Brinell of 37.0 [-]

F

EN 573-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 6000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 6000 Series Aluminium

Shear modulus

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

F

EN 573-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

100 °C, 20 °C

2.3399999999999996e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K

F

EN 573-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Melting point

615.0 - 655.0 °C

Show Material materials with Melting point of 615.0 - 655.0 °C

F

EN 573-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Specific heat capacity

887.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 887.0 - 963.0 J/(kg·K)

Typical for Wrought 6000 Series Aluminium

Thermal conductivity

193.0 - 218.0 W/(m·K)

Show Material materials with Thermal conductivity of 193.0 - 218.0 W/(m·K)

F

EN 573-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Electrical

PropertyValueConditionRelated StandardsShape

Electrical conductivity

29000000.0 - 34000000.0 S/m

Show Material materials with Electrical conductivity of 29000000.0 - 34000000.0 S/m

F

EN 573-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Electrical resistivity

2.94e-08 - 3.45e-08 Ω·m

Show Material materials with Electrical resistivity of 2.94e-08 - 3.45e-08 Ω·m

F

EN 573-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

F

EN 573-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Copper

0.1 %

Show Material materials with Copper of 0.1 %

F

EN 573-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Iron

0.35 %

Show Material materials with Iron of 0.35 %

F

EN 573-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Magnesium

0.45 - 0.9 %

Show Material materials with Magnesium of 0.45 - 0.9 %

F

EN 573-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Manganese

0.1 %

Show Material materials with Manganese of 0.1 %

F

EN 573-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Silicon

0.2 - 0.6 %

Show Material materials with Silicon of 0.2 - 0.6 %

F

EN 573-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Titanium

0.1 %

Show Material materials with Titanium of 0.1 %

F

EN 573-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Zinc

0.1 %

Show Material materials with Zinc of 0.1 %

F

EN 573-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Technological properties

Property
Anodizing

decorative: acceptable, Protective: very good

Brazing

hard brazing (with flux/ without flux): acceptable to poor / sufficient, friction soldering: good, soft brazing with flux: acceptable

Corrosion properties

Seawater: good to acceptable, weathering: good

Workability