EN 573-3 Grade AW-1200 H26

Want to keep this datasheet? Save it now in your required format

Description

Material EN AW-Al 99,0 is produced in large quantities for sheets, strips, plates, scraps, foils, for presswork components, rolled and pressed bars, for prematerial for heat exchanger. It is used in limited quantities for wire and prewire for mechanical application. It is food-safe. The material is comparable to trademark Al 99, material number 3.0205, acc. to DIN 1712-3 : 1976-12. It is well anodizable and shows favorable electrical and thermal conductivity. Smearing may occur on machining. Low mechanical strength, high strain. Formability as well as chemical and weathering resistance are excellent. This material is well suitable for welding and hard soldering. Application: apparatus engineering, roll bond, Z-bond, household appliances, storage and transport equipment for chemical, pharmaceutical and food industry, roofings, facings, arts-and-crafts, packagings, extruded parts, e.g. collapsible tubes, tubes, cans, bottles as well as for hardware and motor vehicle registration plates.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey,Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

2.71 - 2.72 g/cm³

Show Material materials with Density of 2.71 - 2.72 g/cm³

23.0 °C

2.69 - 2.71 g/cm³

Show Material materials with Density of 2.69 - 2.71 g/cm³

Dimension

PropertyValue

Thickness

0.2 - 200 mm

Show Material materials with Thickness of 0.2 - 200 mm

Mechanical

PropertyTemperatureValueComment

Bending angle 90°

23.0 °C

0.5 - 1.5 °/t

Show Material materials with Bending angle 90° of 0.5 - 1.5 °/t

Elastic modulus

20.0 °C

60 - 69 GPa

Show Material materials with Elastic modulus of 60 - 69 GPa

23.0 °C

69 - 70 GPa

Show Material materials with Elastic modulus of 69 - 70 GPa

Unlock all property charts

Elongation A100

20.0 °C

1 - 2 %

Show Material materials with Elongation A100 of 1 - 2 %

Elongation A50

20.0 °C

1 - 4 %

Show Material materials with Elongation A50 of 1 - 4 %

23.0 °C

1 - 4 %

Show Material materials with Elongation A50 of 1 - 4 %

Unlock all property charts

Elongation A50, transverse

20.0 °C

2 - 3 %

Show Material materials with Elongation A50, transverse of 2 - 3 %

Hardness, Brinell

20.0 °C

41 [-]

Show Material materials with Hardness, Brinell of 41 [-]

23.0 °C

41 [-]

Show Material materials with Hardness, Brinell of 41 [-]

Unlock all property charts

Hardness, HBW

23.0 °C

30 - 41 [-]

Show Material materials with Hardness, HBW of 30 - 41 [-]

Plane-Strain Fracture Toughnes

23.0 °C

22 - 35 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Shear modulus

20.0 °C

24 - 26 GPa

Show Material materials with Shear modulus of 24 - 26 GPa

23.0 °C

25.9 - 26.5 GPa

Show Material materials with Shear modulus of 25.9 - 26.5 GPa

Unlock all property charts

Tensile strength

20.0 °C

125 - 180 MPa

Show Material materials with Tensile strength of 125 - 180 MPa

23.0 °C

90 - 180 MPa

Show Material materials with Tensile strength of 90 - 180 MPa

Unlock all property charts

Tensile strength, transverse

20.0 °C

130 - 170 MPa

Show Material materials with Tensile strength, transverse of 130 - 170 MPa

Yield strength

23.0 °C

65 - 105 MPa

Show Material materials with Yield strength of 65 - 105 MPa

Yield strength Rp0.2

20.0 °C

105 MPa

Show Material materials with Yield strength Rp0.2 of 105 MPa

23.0 °C

105 MPa

Show Material materials with Yield strength Rp0.2 of 105 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

105 MPa

Show Material materials with Yield strength Rp0.2, transverse of 105 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-50.0 °C

2.17E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.17E-5 1/K

20-100°C

20.0 °C

2.17E-5 - 2.54E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.17E-5 - 2.54E-5 1/K

20-100°C

100.0 °C

2.35E-5 - 2.4E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.35E-5 - 2.4E-5 1/K

20-100°C

200.0 °C

2.44E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.44E-5 1/K

20-100°C

300.0 °C

2.54E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.54E-5 1/K

20-100°C

Unlock all property charts

Melting point

644 - 657 °C

Show Material materials with Melting point of 644 - 657 °C

Specific heat capacity

20.0 °C

898 J/(kg·K)

Show Material materials with Specific heat capacity of 898 J/(kg·K)

Thermal conductivity

20.0 °C

205 - 225 W/(m·K)

Show Material materials with Thermal conductivity of 205 - 225 W/(m·K)

23.0 °C

138 - 210 W/(m·K)

Show Material materials with Thermal conductivity of 138 - 210 W/(m·K)

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical conductivity

20.0 °C

3.44E+7 - 3.55E+7 S/m

Show Material materials with Electrical conductivity of 3.44E+7 - 3.55E+7 S/m

23.0 °C

3.30E+7 - 3.40E+7 S/m

Show Material materials with Electrical conductivity of 3.30E+7 - 3.40E+7 S/m

Unlock all property charts

Electrical resistivity

20.0 °C

2.95E-8 Ω·m

Show Material materials with Electrical resistivity of 2.95E-8 Ω·m

23.0 °C

2.94E-8 - 4.9E-8 Ω·m

Show Material materials with Electrical resistivity of 2.94E-8 - 4.9E-8 Ω·m

Unlock all property charts

Chemical properties

PropertyValueComment

Aluminium

99 %

Show Material materials with Aluminium of 99 %

Copper

0.05 %

Show Material materials with Copper of 0.05 %

Iron

1 %

Show Material materials with Iron of 1 %

Si + Fe

Manganese

0.05 %

Show Material materials with Manganese of 0.05 %

Other

0.15 %

Show Material materials with Other of 0.15 %

Si + Fe < 1.00, each 0.05, total 0.15

Silicon

1 %

Show Material materials with Silicon of 1 %

Si + Fe

Titanium

0.05 %

Show Material materials with Titanium of 0.05 %

Zinc

0.1 %

Show Material materials with Zinc of 0.1 %

Technological properties

Property
Anodizing

decorative: acceptable, Protective: very good

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels; Roofing: Foil for bituminous coating; Doors: Sheets for composites/ sandwich Panels; Electronic devices: Housing of devices; Heat exchangers: Fins; Cable wrapping: Electric cable wrapping; Insulation; Solar: Solar collectors; Semi-rigid and corrugated: Smooth wall

Brazing

hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good

Corrosion properties

Seawater: sufficient, weathering: acceptable

Welding

Excellent

Workability

Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H12) / very good (H12)