EN 573-3 Grade AW-1050A H16

Want to keep this datasheet? Save it now in your required format

Description

Material EN AW-Al 99,5 is produced in large quantities for sheets, strips, plates, scraps, foils, for presswork components, rolled and pressed bars, for prematerial for heat exchanger as well as for wire and prewire for mechanical and welding application. It is used in limited quantities for prematerial for cans, caps and fasteners as well as for forged parts and prematerial. It is food-safe. The material is comparable to trademark Al 99,5, material number 3.0255, acc. to DIN 1712-3 : 1976-12. It is well anodizable and shows favorable electrical and thermal conductivity. Smearing may occur on machining. Low mechanical strength, high strain. Formability as well as chemical and weathering resistance are excellent. This material is well suitable for welding and hard soldering. Application: apparatus engineering, roll bond, Z-bond, household appliances, storage and transport equipment for chemical, pharmaceutical and food industry, roofings, facings, arts-and-crafts, packagings, extruded parts, e.g. collapsible tubes, tubes, cans, bottles. Furthermore for reflectors, metal signs, large bottles (up to 10 liter), hardware, heat exchanger, pressure vessels, for parts in air fractionation, for heat insulation, aerials, parabolic reflectors, tank and bulk-tank vehicles, body parts, for aircraft construction, tools, moldings and appliances in machine engineering.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

23.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

Mechanical

PropertyTemperatureValueComment

Bending angle 90°

23.0 °C

0.5 - 1.5 °/t

Show Material materials with Bending angle 90° of 0.5 - 1.5 °/t

Elastic modulus

-270.0 °C

70 GPa

Show Material materials with Elastic modulus of 70 GPa

-195.0 °C

78.4 GPa

Show Material materials with Elastic modulus of 78.4 GPa

-85.0 °C

73.5 GPa

Show Material materials with Elastic modulus of 73.5 GPa

-30.0 °C

71.4 GPa

Show Material materials with Elastic modulus of 71.4 GPa

20.0 °C

60 - 70 GPa

Show Material materials with Elastic modulus of 60 - 70 GPa

23.0 °C

69 GPa

Show Material materials with Elastic modulus of 69 GPa

50.0 °C

69 GPa

Show Material materials with Elastic modulus of 69 GPa

100.0 °C

68 - 68.6 GPa

Show Material materials with Elastic modulus of 68 - 68.6 GPa

150.0 °C

66 - 66.5 GPa

Show Material materials with Elastic modulus of 66 - 66.5 GPa

200.0 °C

63 GPa

Show Material materials with Elastic modulus of 63 GPa

250.0 °C

56 - 57 GPa

Show Material materials with Elastic modulus of 56 - 57 GPa

300.0 °C

50 GPa

Show Material materials with Elastic modulus of 50 GPa

Unlock all property charts

Elongation

20.0 °C

4 %

Show Material materials with Elongation of 4 %

23.0 °C

3 %

Show Material materials with Elongation of 3 %

Unlock all property charts

Elongation A100

20.0 °C

1 - 3 %

Show Material materials with Elongation A100 of 1 - 3 %

23.0 °C

4 %

Show Material materials with Elongation A100 of 4 %

Unlock all property charts

Elongation A50

20.0 °C

1 - 3 %

Show Material materials with Elongation A50 of 1 - 3 %

23.0 °C

1 - 3 %

Show Material materials with Elongation A50 of 1 - 3 %

Unlock all property charts

Elongation A50, transverse

20.0 °C

1 - 3 %

Show Material materials with Elongation A50, transverse of 1 - 3 %

Hardness, Brinell

20.0 °C

35 - 39 [-]

Show Material materials with Hardness, Brinell of 35 - 39 [-]

23.0 °C

39 [-]

Show Material materials with Hardness, Brinell of 39 [-]

Unlock all property charts

Plane-Strain Fracture Toughnes

23.0 °C

22 - 35 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Shear modulus

20.0 °C

25 - 26.5 GPa

Show Material materials with Shear modulus of 25 - 26.5 GPa

23.0 °C

25.9 GPa

Show Material materials with Shear modulus of 25.9 GPa

Unlock all property charts

Tensile strength

20.0 °C

120 - 160 MPa

Show Material materials with Tensile strength of 120 - 160 MPa

23.0 °C

120 - 160 MPa

Show Material materials with Tensile strength of 120 - 160 MPa

Unlock all property charts

Tensile strength, transverse

20.0 °C

120 - 160 MPa

Show Material materials with Tensile strength, transverse of 120 - 160 MPa

Yield strength Rp0.2

20.0 °C

100 - 115 MPa

Show Material materials with Yield strength Rp0.2 of 100 - 115 MPa

23.0 °C

100 - 115 MPa

Show Material materials with Yield strength Rp0.2 of 100 - 115 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

100 MPa

Show Material materials with Yield strength Rp0.2, transverse of 100 MPa

Thermal

PropertyTemperatureValue

Coefficient of thermal expansion

-50.0 °C

2.17E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.17E-5 1/K

20.0 °C

2.17E-5 - 2.54E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.17E-5 - 2.54E-5 1/K

100.0 °C

2.35E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.35E-5 1/K

200.0 °C

2.44E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.44E-5 1/K

300.0 °C

2.54E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.54E-5 1/K

Unlock all property charts

Melting point

646 - 657 °C

Show Material materials with Melting point of 646 - 657 °C

Specific heat capacity

20.0 °C

899 - 900 J/(kg·K)

Show Material materials with Specific heat capacity of 899 - 900 J/(kg·K)

23.0 °C

900 J/(kg·K)

Show Material materials with Specific heat capacity of 900 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

210 - 229 W/(m·K)

Show Material materials with Thermal conductivity of 210 - 229 W/(m·K)

23.0 °C

210 - 220 W/(m·K)

Show Material materials with Thermal conductivity of 210 - 220 W/(m·K)

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical conductivity

20.0 °C

3.48E+7 - 3.60E+7 S/m

Show Material materials with Electrical conductivity of 3.48E+7 - 3.60E+7 S/m

23.0 °C

3.40E+7 - 3.60E+7 S/m

Show Material materials with Electrical conductivity of 3.40E+7 - 3.60E+7 S/m

Unlock all property charts

Electrical resistivity

20.0 °C

2.8E-8 - 2.9E-8 Ω·m

Show Material materials with Electrical resistivity of 2.8E-8 - 2.9E-8 Ω·m

23.0 °C

2.78E-8 - 2.94E-8 Ω·m

Show Material materials with Electrical resistivity of 2.78E-8 - 2.94E-8 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Aluminium

99.5 %

Show Material materials with Aluminium of 99.5 %

Boron

0.05 %

Show Material materials with Boron of 0.05 %

Chromium

0.01 %

Show Material materials with Chromium of 0.01 %

Copper

0.05 %

Show Material materials with Copper of 0.05 %

Gallium

0.03 %

Show Material materials with Gallium of 0.03 %

Iron

0.4 %

Show Material materials with Iron of 0.4 %

Magnesium

0.03 - 0.05 %

Show Material materials with Magnesium of 0.03 - 0.05 %

Manganese

0.01 - 0.05 %

Show Material materials with Manganese of 0.01 - 0.05 %

Nickel

0.03 %

Show Material materials with Nickel of 0.03 %

Other

each 0.03

Silicon

0.1 - 0.25 %

Show Material materials with Silicon of 0.1 - 0.25 %

Titanium

0.03 - 0.05 %

Show Material materials with Titanium of 0.03 - 0.05 %

Vanadium

0.03 %

Show Material materials with Vanadium of 0.03 %

Zinc

0.05 - 0.07 %

Show Material materials with Zinc of 0.05 - 0.07 %

Technological properties

Property
Anodizing

decorative: gut (EQ: sehr gut), Protective: very good

Brazing

hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good

Corrosion properties

Seawater: acceptable, weathering: good

Workability

Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H14) / very good (H12)