EN 573-3 Grade AW-6082 T61

Want to keep this datasheet? Save it now in your required format

Description

Age-hardenable AlMgSi alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

20.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

T61

EN 573-3

Flat, Plate, Sheet

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

T61

EN 573-3, EN 1386, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending angle 90°

7.0 °/t

Show Material materials with Bending angle 90° of 7.0 °/t

T61

EN 573-3, EN 1386

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

2.0 °/t

Show Material materials with Bending angle 90° of 2.0 °/t

T61

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

5.0 °/t

Show Material materials with Bending angle 90° of 5.0 °/t

T61

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

2.5 °/t

Show Material materials with Bending angle 90° of 2.5 °/t

T61

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

4.0 °/t

Show Material materials with Bending angle 90° of 4.0 °/t

T61

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

Elastic modulus

20.0 °C

68.0 - 73.0 GPa

Show Material materials with Elastic modulus of 68.0 - 73.0 GPa

T61

EN 573-3

Flat, Plate, Sheet

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

T61

EN 573-3, EN 1386, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

Elongation

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

T61

EN 573-3

Flat

A50 Transverse

20.0 °C

11.0 %

Show Material materials with Elongation of 11.0 %

T61

EN 573-3

Flat

A50 Transverse

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

T61

EN 573-3

Flat

A50 Transverse

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

T61

EN 573-3

Flat

Transverse

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

T61

EN 573-3

Flat

Transverse

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

T61

EN 573-3

Flat

Transverse

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T61

EN 573-3

Flat

Transverse

9.0 %

Show Material materials with Elongation of 9.0 %

T61

EN 573-3, EN 1386

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A50

3.0 %

Show Material materials with Elongation of 3.0 %

T61

EN 573-3, EN 1386

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A50

4.0 %

Show Material materials with Elongation of 4.0 %

T61

EN 573-3, EN 1386

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A50

6.0 %

Show Material materials with Elongation of 6.0 %

T61

EN 573-3, EN 1386

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A50

10.0 %

Show Material materials with Elongation of 10.0 %

T61

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A50

12.0 %

Show Material materials with Elongation of 12.0 %

T61

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A50

11.0 %

Show Material materials with Elongation of 11.0 %

T61

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A50

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

T61

EN 573-3

Plate

A50

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

T61

EN 573-3

Plate

A50

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

T61

EN 573-3

Plate

A50

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

T61

EN 573-3

Plate

A50

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

T61

EN 573-3

Flat

A50

20.0 °C

11.0 %

Show Material materials with Elongation of 11.0 %

T61

EN 573-3

Flat

A50

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

T61

EN 573-3

Flat

A50

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

T61

EN 573-3

Plate, Sheet

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

T61

EN 573-3

Flat

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

T61

EN 573-3

Sheet

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T61

EN 573-3

Sheet

9.0 %

Show Material materials with Elongation of 9.0 %

T61

EN 573-3, EN 1386

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

A100

Hardness, Brinell

82.0 [-]

Show Material materials with Hardness, Brinell of 82.0 [-]

T61

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

20.0 °C

82.0 [-]

Show Material materials with Hardness, Brinell of 82.0 [-]

T61

EN 573-3

Flat

20.0 °C

81.0 - 82.0 [-]

Show Material materials with Hardness, Brinell of 81.0 - 82.0 [-]

T61

EN 573-3

Flat

20.0 °C

81.0 [-]

Show Material materials with Hardness, Brinell of 81.0 [-]

T61

EN 573-3

Flat, Sheet

Unlock all property charts

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 6000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 6000 Series Aluminium

Shear modulus

20.0 °C

26.0 - 27.0 GPa

Show Material materials with Shear modulus of 26.0 - 27.0 GPa

T61

EN 573-3

Flat, Plate, Sheet

26.4 GPa

Show Material materials with Shear modulus of 26.4 GPa

T61

EN 573-3, EN 1386, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

Tensile strength

20.0 °C

280.0 MPa

Show Material materials with Tensile strength of 280.0 MPa

T61

EN 573-3

Flat

Transverse

20.0 °C

275.0 MPa

Show Material materials with Tensile strength of 275.0 MPa

T61

EN 573-3

Flat

Transverse

280.0 MPa

Show Material materials with Tensile strength of 280.0 MPa

T61

EN 573-3, EN 1386, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

20.0 °C

280.0 MPa

Show Material materials with Tensile strength of 280.0 MPa

T61

EN 573-3

Plate, Flat

20.0 °C

275.0 MPa

Show Material materials with Tensile strength of 275.0 MPa

T61

EN 573-3

Sheet, Flat

Unlock all property charts

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

100 °C, 20 °C

2.3399999999999996e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K

T61

EN 573-3, EN 1386, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

Melting point

585.0 - 650.0 °C

Show Material materials with Melting point of 585.0 - 650.0 °C

T61

EN 573-3, EN 1386, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

Specific heat capacity

896.0 J/(kg·K)

Show Material materials with Specific heat capacity of 896.0 J/(kg·K)

T61

EN 573-3, EN 1386, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

Thermal conductivity

20.0 °C

170.0 - 220.0 W/(m·K)

Show Material materials with Thermal conductivity of 170.0 - 220.0 W/(m·K)

T61

EN 573-3, EN 1386, EN 485

Flat, Plate, Sheet, Strip, Wire, Forging, Tube, Bar

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

24000000.0 - 32000000.0 S/m

Show Material materials with Electrical conductivity of 24000000.0 - 32000000.0 S/m

T61

EN 573-3, EN 1386, EN 485

Flat, Plate, Sheet, Strip, Wire, Forging, Tube, Bar

Electrical resistivity

3.13e-08 - 4.17e-08 Ω·m

Show Material materials with Electrical resistivity of 3.13e-08 - 4.17e-08 Ω·m

T61

EN 573-3, EN 1386, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.25 %

Show Material materials with Chromium of 0.25 %

T61

EN 573-3, EN 1386, EN 485

Flat, Plate, Sheet, Strip, Wire, Forging, Tube, Bar

Copper

0.1 %

Show Material materials with Copper of 0.1 %

T61

EN 573-3, EN 1386, EN 485

Flat, Plate, Sheet, Strip, Wire, Forging, Tube, Bar

Iron

0.5 %

Show Material materials with Iron of 0.5 %

T61

EN 573-3

Flat, Plate, Sheet

0.50 %

Show Material materials with Iron of 0.50 %

T61

EN 573-3, EN 1386, EN 485

Strip, Sheet, Plate, Wire, Forging, Tube, Bar

Magnesium

0.6 - 1.2 %

Show Material materials with Magnesium of 0.6 - 1.2 %

T61

EN 573-3, EN 1386, EN 485

Flat, Plate, Sheet, Strip, Wire, Forging, Tube, Bar

Manganese

0.4 - 1.0 %

Show Material materials with Manganese of 0.4 - 1.0 %

T61

EN 573-3, EN 1386, EN 485

Flat, Plate, Sheet, Strip, Wire, Forging, Tube, Bar

Silicon

0.7 - 1.3 %

Show Material materials with Silicon of 0.7 - 1.3 %

T61

EN 573-3, EN 1386, EN 485

Flat, Plate, Sheet, Strip, Wire, Forging, Tube, Bar

Titanium

0.1 %

Show Material materials with Titanium of 0.1 %

T61

EN 573-3, EN 1386, EN 485

Flat, Plate, Sheet, Strip, Wire, Forging, Tube, Bar

Zinc

0.2 %

Show Material materials with Zinc of 0.2 %

T61

EN 573-3, EN 1386, EN 485

Flat, Plate, Sheet, Strip, Wire, Forging, Tube, Bar

Technological properties

Property
Anodizing

decorative: acceptable, Protective: very good

Brazing

hard brazing (with flux/ without flux): good / sufficient, friction soldering: good, soft brazing with flux: acceptable

Corrosion properties

Seawater: good, weathering: very good

Workability

Bending / Spinning (cold): acceptable (T3, T4) / good (O), Impact extrusion (cold): good (O), Deep drawing / upsetting (Condition) good (O) / good (O)