EN 573-3 Grade AW-7010 T652

Want to keep this datasheet? Save it now in your required format

Description

Age-hardenable AlZn alloy. The alloy is not food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated StandardsShape

Density

2.82 g/cm³

Show Material materials with Density of 2.82 g/cm³

T652

EN 573-3, EN 485

Strip, Sheet, Plate

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending angle 90°

12.0 °/t

Show Material materials with Bending angle 90° of 12.0 °/t

T652

EN 573-3, EN 485

Strip, Sheet, Plate

Elastic modulus

72.0 GPa

Show Material materials with Elastic modulus of 72.0 GPa

T652

EN 573-3, EN 485

Strip, Sheet, Plate

Elongation

1.0 %

Show Material materials with Elongation of 1.0 %

T652

EN 573-3, EN 485

Strip, Sheet, Plate

A100

2.0 %

Show Material materials with Elongation of 2.0 %

T652

EN 573-3, EN 485

Strip, Sheet, Plate

A100

4.0 %

Show Material materials with Elongation of 4.0 %

T652

EN 573-3, EN 485

Strip, Sheet, Plate

A100

5.0 %

Show Material materials with Elongation of 5.0 %

T652

EN 573-3, EN 485

Strip, Sheet, Plate

A100

6.0 %

Show Material materials with Elongation of 6.0 %

T652

EN 573-3, EN 485

Strip, Sheet, Plate

A100

20.0 °C

1.0 %

Show Material materials with Elongation of 1.0 %

T652

EN 573-3

Flat

Transverse

20.0 °C

1.0 %

Show Material materials with Elongation of 1.0 %

T652

EN 573-3

Sheet

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

T652

EN 573-3

Flat

Transverse

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

T652

EN 573-3

Sheet

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

T652

EN 573-3

Flat

Transverse

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

T652

EN 573-3

Sheet

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

T652

EN 573-3

Flat

Transverse

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

T652

EN 573-3

Sheet

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

T652

EN 573-3

Flat

Transverse

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

T652

EN 573-3

Flat

Hardness, Brinell

20.0 °C

175.0 - 190.0 [-]

Show Material materials with Hardness, Brinell of 175.0 - 190.0 [-]

T652

EN 573-3

Flat

20.0 °C

175.0 - 185.0 [-]

Show Material materials with Hardness, Brinell of 175.0 - 185.0 [-]

T652

EN 573-3

Flat, Sheet

20.0 °C

175.0 - 180.0 [-]

Show Material materials with Hardness, Brinell of 175.0 - 180.0 [-]

T652

EN 573-3

Flat, Sheet

20.0 °C

175.0 [-]

Show Material materials with Hardness, Brinell of 175.0 [-]

T652

EN 573-3

Flat, Sheet

20.0 °C

180.0 - 190.0 [-]

Show Material materials with Hardness, Brinell of 180.0 - 190.0 [-]

T652

EN 573-3

Flat

20.0 °C

180.0 - 185.0 [-]

Show Material materials with Hardness, Brinell of 180.0 - 185.0 [-]

T652

EN 573-3

Flat, Sheet

20.0 °C

180.0 [-]

Show Material materials with Hardness, Brinell of 180.0 [-]

T652

EN 573-3

Flat, Sheet

20.0 °C

185.0 - 190.0 [-]

Show Material materials with Hardness, Brinell of 185.0 - 190.0 [-]

T652

EN 573-3

Flat

20.0 °C

185.0 [-]

Show Material materials with Hardness, Brinell of 185.0 [-]

T652

EN 573-3

Flat, Sheet

20.0 °C

190.0 [-]

Show Material materials with Hardness, Brinell of 190.0 [-]

T652

EN 573-3

Flat

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 7000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 7000 Series Aluminium

Shear modulus

27.1 GPa

Show Material materials with Shear modulus of 27.1 GPa

T652

EN 573-3, EN 485

Strip, Sheet, Plate

Tensile strength

470.0 MPa

Show Material materials with Tensile strength of 470.0 MPa

T652

EN 573-3, EN 485

Strip, Sheet, Plate

505.0 MPa

Show Material materials with Tensile strength of 505.0 MPa

T652

EN 573-3, EN 485

Strip, Sheet, Plate

525.0 MPa

Show Material materials with Tensile strength of 525.0 MPa

T652

EN 573-3, EN 485

Strip, Sheet, Plate

540.0 MPa

Show Material materials with Tensile strength of 540.0 MPa

T652

EN 573-3, EN 485

Strip, Sheet, Plate

550.0 MPa

Show Material materials with Tensile strength of 550.0 MPa

T652

EN 573-3, EN 485

Strip, Sheet, Plate

560.0 MPa

Show Material materials with Tensile strength of 560.0 MPa

T652

EN 573-3, EN 485

Strip, Sheet, Plate

570.0 MPa

Show Material materials with Tensile strength of 570.0 MPa

T652

EN 573-3, EN 485

Strip, Sheet, Plate

20.0 °C

470.0 MPa

Show Material materials with Tensile strength of 470.0 MPa

T652

EN 573-3

Flat

Transverse

20.0 °C

470.0 MPa

Show Material materials with Tensile strength of 470.0 MPa

T652

EN 573-3

Sheet

20.0 °C

505.0 MPa

Show Material materials with Tensile strength of 505.0 MPa

T652

EN 573-3

Flat

Transverse

20.0 °C

505.0 MPa

Show Material materials with Tensile strength of 505.0 MPa

T652

EN 573-3

Sheet

20.0 °C

525.0 MPa

Show Material materials with Tensile strength of 525.0 MPa

T652

EN 573-3

Flat

Transverse

20.0 °C

525.0 MPa

Show Material materials with Tensile strength of 525.0 MPa

T652

EN 573-3

Sheet

20.0 °C

540.0 MPa

Show Material materials with Tensile strength of 540.0 MPa

T652

EN 573-3

Flat

Transverse

20.0 °C

540.0 MPa

Show Material materials with Tensile strength of 540.0 MPa

T652

EN 573-3

Sheet

20.0 °C

550.0 MPa

Show Material materials with Tensile strength of 550.0 MPa

T652

EN 573-3

Flat

Transverse

20.0 °C

550.0 MPa

Show Material materials with Tensile strength of 550.0 MPa

T652

EN 573-3

Sheet

20.0 °C

560.0 MPa

Show Material materials with Tensile strength of 560.0 MPa

T652

EN 573-3

Flat

Transverse

20.0 °C

560.0 MPa

Show Material materials with Tensile strength of 560.0 MPa

T652

EN 573-3

Sheet

20.0 °C

570.0 MPa

Show Material materials with Tensile strength of 570.0 MPa

T652

EN 573-3

Flat

Transverse

20.0 °C

570.0 MPa

Show Material materials with Tensile strength of 570.0 MPa

T652

EN 573-3

Flat

Thermal

PropertyValueComment

Coefficient of thermal expansion

2.1e-05 - 2.4e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.1e-05 - 2.4e-05 1/K

Typical for Wrought 7000 Series Aluminium

Melting point

465.0 - 655.0 °C

Show Material materials with Melting point of 465.0 - 655.0 °C

Typical for Wrought 7000 Series Aluminium

Specific heat capacity

795.0 - 1050.0 J/(kg·K)

Show Material materials with Specific heat capacity of 795.0 - 1050.0 J/(kg·K)

Typical for Wrought 7000 Series Aluminium

Thermal conductivity

121.0 - 170.0 W/(m·K)

Show Material materials with Thermal conductivity of 121.0 - 170.0 W/(m·K)

Typical for Wrought 7000 Series Aluminium

Electrical

PropertyValueComment

Electrical conductivity

18000000.0 - 34000000.0 S/m

Show Material materials with Electrical conductivity of 18000000.0 - 34000000.0 S/m

Typical for Wrought 7000 Series Aluminium

Electrical resistivity

2.9e-08 - 5.6e-08 Ω·m

Show Material materials with Electrical resistivity of 2.9e-08 - 5.6e-08 Ω·m

Typical for Wrought 7000 Series Aluminium

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.05 %

Show Material materials with Chromium of 0.05 %

T652

EN 573-3, EN 485

Flat, Sheet, Strip, Plate

Copper

1.5 - 2.0 %

Show Material materials with Copper of 1.5 - 2.0 %

T652

EN 573-3, EN 485

Flat, Sheet, Strip, Plate

Iron

0.15 %

Show Material materials with Iron of 0.15 %

T652

EN 573-3

Flat, Sheet

0.15 %

Show Material materials with Iron of 0.15 %

T652

EN 573-3, EN 485

Strip, Sheet, Plate

Magnesium

2.1 - 2.6 %

Show Material materials with Magnesium of 2.1 - 2.6 %

T652

EN 573-3, EN 485

Flat, Sheet, Strip, Plate

Manganese

0.1 %

Show Material materials with Manganese of 0.1 %

T652

EN 573-3, EN 485

Flat, Sheet, Strip, Plate

Nickel

0.05 %

Show Material materials with Nickel of 0.05 %

T652

EN 573-3, EN 485

Flat, Sheet, Strip, Plate

Silicon

0.12 %

Show Material materials with Silicon of 0.12 %

T652

EN 573-3, EN 485

Flat, Sheet, Strip, Plate

Titanium

0.06 %

Show Material materials with Titanium of 0.06 %

T652

EN 573-3, EN 485

Flat, Sheet, Strip, Plate

Zinc

5.7 - 6.7 %

Show Material materials with Zinc of 5.7 - 6.7 %

T652

EN 573-3, EN 485

Flat, Sheet, Strip, Plate

Zirconium

0.1 - 0.16 %

Show Material materials with Zirconium of 0.1 - 0.16 %

T652

EN 573-3, EN 485

Flat, Sheet, Strip, Plate

Technological properties

Property
Brazing

Excellent