EN 573-3 Grade AW-1050A F

Want to keep this datasheet? Save it now in your required format

Description

Food safe aluminum.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

-270.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

-195.0 °C

78.4 GPa

Show Material materials with Elastic modulus of 78.4 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

-85.0 °C

73.5 GPa

Show Material materials with Elastic modulus of 73.5 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

-30.0 °C

71.4 GPa

Show Material materials with Elastic modulus of 71.4 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

60.0 - 70.0 GPa

Show Material materials with Elastic modulus of 60.0 - 70.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

20.0 °C

60.0 - 69.0 GPa

Show Material materials with Elastic modulus of 60.0 - 69.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

20.0 °C

69.0 - 70.0 GPa

Show Material materials with Elastic modulus of 69.0 - 70.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

20.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

50.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

100.0 °C

68.0 GPa

Show Material materials with Elastic modulus of 68.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube

100.0 °C

68.0 - 68.6 GPa

Show Material materials with Elastic modulus of 68.0 - 68.6 GPa

F

EN 573-3

Profile, Rod, Flat, Tube

100.0 °C

68.6 GPa

Show Material materials with Elastic modulus of 68.6 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

150.0 °C

66.0 GPa

Show Material materials with Elastic modulus of 66.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube

150.0 °C

66.0 - 66.5 GPa

Show Material materials with Elastic modulus of 66.0 - 66.5 GPa

F

EN 573-3

Profile, Rod, Flat, Tube

150.0 °C

66.5 GPa

Show Material materials with Elastic modulus of 66.5 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

200.0 °C

63.0 GPa

Show Material materials with Elastic modulus of 63.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

250.0 °C

56.0 - 57.0 GPa

Show Material materials with Elastic modulus of 56.0 - 57.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube

250.0 °C

56.0 GPa

Show Material materials with Elastic modulus of 56.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

250.0 °C

57.0 GPa

Show Material materials with Elastic modulus of 57.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube

300.0 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

F

EN 573-3

Profile, Rod, Flat, Tube

Elongation

23.0 %

Show Material materials with Elongation of 23.0 %

F

EN 573-3, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

25.0 %

Show Material materials with Elongation of 25.0 %

F

EN 573-3, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A100

20.0 °C

23.0 %

Show Material materials with Elongation of 23.0 %

F

EN 573-3

Profile, Rod, Tube

A50

20.0 °C

25.0 %

Show Material materials with Elongation of 25.0 %

F

EN 573-3

Profile, Rod, Tube

Hardness, Brinell

23.0 [-]

Show Material materials with Hardness, Brinell of 23.0 [-]

F

EN 573-3, EN 570

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

20.0 [-]

Show Material materials with Hardness, Brinell of 20.0 [-]

F

EN 573-3

Profile, Rod, Tube

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

Shear modulus

25.9 GPa

Show Material materials with Shear modulus of 25.9 GPa

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

25.0 - 26.5 GPa

Show Material materials with Shear modulus of 25.0 - 26.5 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

20.0 °C

25.0 - 25.9 GPa

Show Material materials with Shear modulus of 25.0 - 25.9 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

20.0 °C

25.9 - 26.5 GPa

Show Material materials with Shear modulus of 25.9 - 26.5 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

20.0 °C

25.9 GPa

Show Material materials with Shear modulus of 25.9 GPa

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

Tensile strength

60.0 MPa

Show Material materials with Tensile strength of 60.0 MPa

F

EN 573-3, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

65.0 MPa

Show Material materials with Tensile strength of 65.0 MPa

F

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

80.0 - 130.0 MPa

Show Material materials with Tensile strength of 80.0 - 130.0 MPa

F

EN 573-3, EN 1715-3, EN 1715-4

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

60.0 MPa

Show Material materials with Tensile strength of 60.0 MPa

F

EN 573-3

Profile, Rod, Tube, Flat

20.0 °C

60.0 MPa

Show Material materials with Tensile strength of 60.0 MPa

F

EN 573-3

Flat

Transverse

20.0 °C

65.0 MPa

Show Material materials with Tensile strength of 65.0 MPa

F

EN 573-3

Flat

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

-50 °C

2.17e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat

-50.0 °C

2.17e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat

20 °C

2.17e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat

20 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat

20 °C

2.4399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4399999999999997e-05 1/K

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20 °C

2.5399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5399999999999997e-05 1/K

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

100 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat

100.0 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat

200 °C

2.4399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4399999999999997e-05 1/K

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

200.0 °C

2.44e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.44e-05 1/K

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

300 °C

2.5399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5399999999999997e-05 1/K

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

300.0 °C

2.54e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.54e-05 1/K

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

Melting point

646.0 - 657.0 °C

Show Material materials with Melting point of 646.0 - 657.0 °C

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Specific heat capacity

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

899.0 - 900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 899.0 - 900.0 J/(kg·K)

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

20.0 °C

899.0 J/(kg·K)

Show Material materials with Specific heat capacity of 899.0 J/(kg·K)

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

20.0 °C

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

Thermal conductivity

20.0 °C

210.0 - 220.0 W/(m·K)

Show Material materials with Thermal conductivity of 210.0 - 220.0 W/(m·K)

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat

20.0 °C

210.0 - 229.0 W/(m·K)

Show Material materials with Thermal conductivity of 210.0 - 229.0 W/(m·K)

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

20.0 °C

220.0 - 229.0 W/(m·K)

Show Material materials with Thermal conductivity of 220.0 - 229.0 W/(m·K)

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

20.0 °C

229.0 W/(m·K)

Show Material materials with Thermal conductivity of 229.0 W/(m·K)

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

34000000.0 - 36000000.0 S/m

Show Material materials with Electrical conductivity of 34000000.0 - 36000000.0 S/m

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

34800000.0 - 36000000.0 S/m

Show Material materials with Electrical conductivity of 34800000.0 - 36000000.0 S/m

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

Electrical resistivity

2.78e-08 - 2.94e-08 Ω·m

Show Material materials with Electrical resistivity of 2.78e-08 - 2.94e-08 Ω·m

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

2.8e-08 - 2.9e-08 Ω·m

Show Material materials with Electrical resistivity of 2.8e-08 - 2.9e-08 Ω·m

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

20.0 °C

2.9e-08 Ω·m

Show Material materials with Electrical resistivity of 2.9e-08 Ω·m

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminium

99.5 %

Show Material materials with Aluminium of 99.5 %

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Bar

Boron

0.05

Show Material materials with Boron of 0.05

F

EN 573-3

Profile, Rod, Flat, Tube

Chromium

0.01

Show Material materials with Chromium of 0.01

F

EN 573-3

Profile, Rod, Flat, Tube

Copper

0.05 %

Show Material materials with Copper of 0.05 %

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Profile, Rod, Flat, Tube, Plate, Strip, Sheet, Foil, Bar

Gallium

0.03

Show Material materials with Gallium of 0.03

F

EN 573-3

Profile, Rod, Flat, Tube

Iron

0.4 %

Show Material materials with Iron of 0.4 %

F

EN 573-3

Profile, Rod, Flat, Tube, Plate

0.40 %

Show Material materials with Iron of 0.40 %

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Magnesium

0.03 %

Show Material materials with Magnesium of 0.03 %

F

EN 573-3

Profile, Rod, Flat, Tube

0.05 %

Show Material materials with Magnesium of 0.05 %

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Profile, Rod, Flat, Tube, Plate, Strip, Sheet, Foil, Bar

Manganese

0.01 %

Show Material materials with Manganese of 0.01 %

F

EN 573-3

Profile, Rod, Flat, Tube

0.05 %

Show Material materials with Manganese of 0.05 %

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Profile, Rod, Flat, Tube, Plate, Strip, Sheet, Foil, Bar

Nickel

0.03

Show Material materials with Nickel of 0.03

F

EN 573-3

Profile, Rod, Flat, Tube

Silicon

0.1 %

Show Material materials with Silicon of 0.1 %

F

EN 573-3

Profile, Rod, Flat, Tube

0.25 %

Show Material materials with Silicon of 0.25 %

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Profile, Rod, Flat, Tube, Plate, Strip, Sheet, Foil, Bar

Titanium

0.03 %

Show Material materials with Titanium of 0.03 %

F

EN 573-3

Profile, Rod, Flat, Tube

0.05 %

Show Material materials with Titanium of 0.05 %

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Profile, Rod, Flat, Tube, Plate, Strip, Sheet, Foil, Bar

Vanadium

0.03

Show Material materials with Vanadium of 0.03

F

EN 573-3

Profile, Rod, Flat, Tube

Zinc

0.05 %

Show Material materials with Zinc of 0.05 %

F

EN 573-3

Profile, Rod, Flat, Tube

0.07 %

Show Material materials with Zinc of 0.07 %

F

EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755

Profile, Rod, Flat, Tube, Plate, Strip, Sheet, Foil, Bar

Technological properties

Property
Anodizing

decorative: gut (EQ: sehr gut), Protective: very good

Brazing

hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good

Corrosion properties

Seawater: acceptable, weathering: good

Workability

Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H14) / very good (H12)