EN 573-3 Grade AW-1070A H18

Want to keep this datasheet? Save it now in your required format

Description

Food safe aluminum.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,Aludium,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.69 g/cm³

Show Material materials with Density of 2.69 g/cm³

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H18

EN 573-3, EN 1301, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

20.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H18

EN 573-3

Flat, Wire

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.2 mm

Show Material materials with Thickness of 0.2 mm

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

0.2 mm

Coil, Sheet, Strip

3 mm

Show Material materials with Thickness of 3 mm

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

3 mm

Coil, Sheet, Strip

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending angle 90°

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

H18

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

2.0 °/t

Show Material materials with Bending angle 90° of 2.0 °/t

H18

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

2.5 °/t

Show Material materials with Bending angle 90° of 2.5 °/t

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

according to EN 485-2

2.5 °/t

Show Material materials with Bending angle 90° of 2.5 °/t

H18

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

Elastic modulus

-270.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H18

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Flat, Wire, Coil, Sheet, Strip

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H18

EN 573-3, EN 1301, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

20.0 °C

60.0 - 70.0 GPa

Show Material materials with Elastic modulus of 60.0 - 70.0 GPa

H18

EN 573-3

Flat, Wire

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H18

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Flat, Wire, Coil, Sheet, Strip

50.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H18

EN 573-3

Flat, Wire

100.0 °C

68.0 GPa

Show Material materials with Elastic modulus of 68.0 GPa

H18

EN 573-3

Flat, Wire

150.0 °C

66.0 GPa

Show Material materials with Elastic modulus of 66.0 GPa

H18

EN 573-3

Flat, Wire

200.0 °C

63.0 GPa

Show Material materials with Elastic modulus of 63.0 GPa

H18

EN 573-3

Flat, Wire

250.0 °C

57.0 GPa

Show Material materials with Elastic modulus of 57.0 GPa

H18

EN 573-3

Flat, Wire

300.0 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

H18

EN 573-3

Flat, Wire

Elongation

2 %

Show Material materials with Elongation of 2 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

according to EN 485-2, A50

2.0 %

Show Material materials with Elongation of 2.0 %

H18

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

A50

3.0 %

Show Material materials with Elongation of 3.0 %

H18

EN 573-3, EN 1301

Strip, Sheet, Plate, Wire, Tube, Bar

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H18

EN 573-3

Flat

A50 Transverse

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H18

EN 573-3

Flat

A50

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

H18

EN 573-3

Wire

A100

Hardness, Brinell

40.0 [-]

Show Material materials with Hardness, Brinell of 40.0 [-]

H18

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

20.0 °C

40.0 [-]

Show Material materials with Hardness, Brinell of 40.0 [-]

H18

EN 573-3

Flat

Hardness, HBW

40 [-]

Show Material materials with Hardness, HBW of 40 [-]

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

according to EN 485-2

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 1000 Series Aluminium

Shear modulus

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

20.0 °C

25.0 - 26.5 GPa

Show Material materials with Shear modulus of 25.0 - 26.5 GPa

H18

EN 573-3

Flat, Wire

Tensile strength

125 MPa

Show Material materials with Tensile strength of 125 MPa

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

according to EN 485-2

125.0 MPa

Show Material materials with Tensile strength of 125.0 MPa

H18

EN 573-3, EN 1301, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

20.0 °C

125.0 MPa

Show Material materials with Tensile strength of 125.0 MPa

H18

EN 573-3

Flat

Transverse

20.0 °C

125.0 MPa

Show Material materials with Tensile strength of 125.0 MPa

H18

EN 573-3

Wire, Flat

Yield strength

105.0 MPa

Show Material materials with Yield strength of 105.0 MPa

H18

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

RP02

105 MPa

Show Material materials with Yield strength of 105 MPa

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

according to EN 485-2

120.0 MPa

Show Material materials with Yield strength of 120.0 MPa

H18

EN 573-3, EN 1301

Strip, Sheet, Plate, Wire, Tube, Bar

RP02

20.0 °C

105.0 MPa

Show Material materials with Yield strength of 105.0 MPa

H18

EN 573-3

Flat

RP02 Transverse

20.0 °C

105.0 MPa

Show Material materials with Yield strength of 105.0 MPa

H18

EN 573-3

Flat

RP02

20.0 °C

125.0 MPa

Show Material materials with Yield strength of 125.0 MPa

H18

EN 573-3

Wire

RP02

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H18

EN 573-3, EN 1301, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

100 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H18

EN 573-3, EN 1301, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

20-100°C

Melting point

659.0 °C

Show Material materials with Melting point of 659.0 °C

H18

EN 573-3, EN 1301, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

Specific heat capacity

20.0 °C

921.0 J/(kg·K)

Show Material materials with Specific heat capacity of 921.0 J/(kg·K)

H18

EN 573-3

Flat, Wire

Thermal conductivity

138 W/(m·K)

Show Material materials with Thermal conductivity of 138 W/(m·K)

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

225 W/(m·K)

Show Material materials with Thermal conductivity of 225 W/(m·K)

H18

EN 573-3, EN 1301, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

20.0 °C

215.0 W/(m·K)

Show Material materials with Thermal conductivity of 215.0 W/(m·K)

H18

EN 573-3

Flat, Wire

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

34500000.0 - 35000000.0 S/m

Show Material materials with Electrical conductivity of 34500000.0 - 35000000.0 S/m

H18

EN 573-3, EN 1301, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

20.0 °C

35800000.0 - 36800000.0 S/m

Show Material materials with Electrical conductivity of 35800000.0 - 36800000.0 S/m

H18

EN 573-3

Flat, Wire

Electrical resistivity

2.86e-08 - 2.9e-08 Ω·m

Show Material materials with Electrical resistivity of 2.86e-08 - 2.9e-08 Ω·m

H18

EN 573-3, EN 1301, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

4.9e-08 Ω·m

Show Material materials with Electrical resistivity of 4.9e-08 Ω·m

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Chemical properties

PropertyValueConditionRelated StandardsShapeComment

Aluminium

99.7 %

Show Material materials with Aluminium of 99.7 %

H18

EN 573-3, EN 1301, EN 485

Flat, Wire, Strip, Sheet, Plate, Tube, Bar

Copper

0.03 %

Show Material materials with Copper of 0.03 %

H18

EN 573-3, EN 1301, EN 485

Flat, Wire, Strip, Sheet, Plate, Tube, Bar

0.03 %

Show Material materials with Copper of 0.03 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Iron

0.25 %

Show Material materials with Iron of 0.25 %

H18

EN 573-3

Flat, Wire

0.25 %

Show Material materials with Iron of 0.25 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3, EN 1301, EN 485

Coil, Sheet, Strip, Strip, Sheet, Plate, Wire, Tube, Bar

Magnesium

0.03 %

Show Material materials with Magnesium of 0.03 %

H18

EN 573-3, EN 1301, EN 485

Flat, Wire, Strip, Sheet, Plate, Tube, Bar

0.03 %

Show Material materials with Magnesium of 0.03 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Manganese

0.03 %

Show Material materials with Manganese of 0.03 %

H18

EN 573-3, EN 1301, EN 485

Flat, Wire, Strip, Sheet, Plate, Tube, Bar

0.03 %

Show Material materials with Manganese of 0.03 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Other

0.03 %

Show Material materials with Other of 0.03 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Min.

Silicon

0.2 %

Show Material materials with Silicon of 0.2 %

H18

EN 573-3, EN 1301, EN 485

Flat, Wire, Strip, Sheet, Plate, Tube, Bar

0.2 %

Show Material materials with Silicon of 0.2 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Titanium

0.03 %

Show Material materials with Titanium of 0.03 %

H18

EN 573-3, EN 1301, EN 485

Flat, Wire, Strip, Sheet, Plate, Tube, Bar

0.03 %

Show Material materials with Titanium of 0.03 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Zinc

0.07 %

Show Material materials with Zinc of 0.07 %

H18

EN 573-3, EN 1301, EN 485

Flat, Wire, Strip, Sheet, Plate, Tube, Bar

0.07 %

Show Material materials with Zinc of 0.07 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Technological properties

Property
Anodizing

Excellent

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels, Foil for bituminous coating; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Lighting: Anodizing Quality, Lacquering quality; Electronic devices: Housing of devices; Tubes: Industrial tubes, Flexible tube, Pipes; Insulation; Solar: Solar collectors, Photovoltaic panels; Wind energy: Nacelle coverings, Rotor, Hub, Stairs; Cosmetics: Cosmetic pieces; Automotive trim: Interior trim, Windows frame, Marque badges

Brazing

hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good

Corrosion properties

Excellent

Welding

Excellent

Workability

Excellent