EN 573-3 Grade AW-1070A F

Want to keep this datasheet? Save it now in your required format

Description

Food safe aluminum.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

F

EN 573-3, EN 1715-3, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Wire, Tube, Bar

20.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

F

EN 573-3

Rod, Flat

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

-270.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

F

EN 573-3

Rod, Flat

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

F

EN 573-3, EN 1715-3, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Wire, Tube, Bar

20.0 °C

60.0 - 70.0 GPa

Show Material materials with Elastic modulus of 60.0 - 70.0 GPa

F

EN 573-3

Rod, Flat

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

F

EN 573-3

Rod, Flat

50.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

F

EN 573-3

Rod, Flat

100.0 °C

68.0 GPa

Show Material materials with Elastic modulus of 68.0 GPa

F

EN 573-3

Rod, Flat

150.0 °C

66.0 GPa

Show Material materials with Elastic modulus of 66.0 GPa

F

EN 573-3

Rod, Flat

200.0 °C

63.0 GPa

Show Material materials with Elastic modulus of 63.0 GPa

F

EN 573-3

Rod, Flat

250.0 °C

57.0 GPa

Show Material materials with Elastic modulus of 57.0 GPa

F

EN 573-3

Rod, Flat

300.0 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

F

EN 573-3

Rod, Flat

Elongation

23.0 %

Show Material materials with Elongation of 23.0 %

F

EN 573-3, EN 755

Strip, Sheet, Plate, Wire, Tube, Bar

A50

25.0 %

Show Material materials with Elongation of 25.0 %

F

EN 573-3, EN 755

Strip, Sheet, Plate, Wire, Tube, Bar

A100

20.0 °C

23.0 %

Show Material materials with Elongation of 23.0 %

F

EN 573-3

Rod

A50

20.0 °C

25.0 %

Show Material materials with Elongation of 25.0 %

F

EN 573-3

Rod

Unlock all property charts

Hardness, Brinell

21.0 [-]

Show Material materials with Hardness, Brinell of 21.0 [-]

F

EN 573-3, EN 570

Strip, Sheet, Plate, Wire, Tube, Bar

20.0 °C

18.0 [-]

Show Material materials with Hardness, Brinell of 18.0 [-]

F

EN 573-3

Rod

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 1000 Series Aluminium

Shear modulus

20.0 °C

25.0 - 26.5 GPa

Show Material materials with Shear modulus of 25.0 - 26.5 GPa

F

EN 573-3

Rod, Flat

Tensile strength

60.0 MPa

Show Material materials with Tensile strength of 60.0 MPa

F

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Wire, Tube, Bar

80.0 - 110.0 MPa

Show Material materials with Tensile strength of 80.0 - 110.0 MPa

F

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Wire, Tube, Bar

20.0 °C

60.0 MPa

Show Material materials with Tensile strength of 60.0 MPa

F

EN 573-3

Rod, Flat

20.0 °C

60.0 MPa

Show Material materials with Tensile strength of 60.0 MPa

F

EN 573-3

Flat

Transverse

Unlock all property charts

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

20 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

F

EN 573-3, EN 1715-3, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Wire, Tube, Bar

100 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

F

EN 573-3, EN 1715-3, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Wire, Tube, Bar

Unlock all property charts

Melting point

659.0 °C

Show Material materials with Melting point of 659.0 °C

F

EN 573-3, EN 1715-3, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Wire, Tube, Bar

Specific heat capacity

20.0 °C

921.0 J/(kg·K)

Show Material materials with Specific heat capacity of 921.0 J/(kg·K)

F

EN 573-3

Rod, Flat

Thermal conductivity

225 W/(m·K)

Show Material materials with Thermal conductivity of 225 W/(m·K)

F

EN 573-3, EN 1715-3, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Wire, Tube, Bar

20.0 °C

215.0 W/(m·K)

Show Material materials with Thermal conductivity of 215.0 W/(m·K)

F

EN 573-3

Rod, Flat

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

34500000.0 - 35000000.0 S/m

Show Material materials with Electrical conductivity of 34500000.0 - 35000000.0 S/m

F

EN 573-3, EN 1715-3, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Wire, Tube, Bar

20.0 °C

35800000.0 - 36800000.0 S/m

Show Material materials with Electrical conductivity of 35800000.0 - 36800000.0 S/m

F

EN 573-3

Rod, Flat

Electrical resistivity

2.86e-08 - 2.9e-08 Ω·m

Show Material materials with Electrical resistivity of 2.86e-08 - 2.9e-08 Ω·m

F

EN 573-3, EN 1715-3, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Wire, Tube, Bar

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminium

99.7 %

Show Material materials with Aluminium of 99.7 %

F

EN 573-3, EN 1715-3, EN 485, EN 570, EN 755

Rod, Flat, Strip, Sheet, Plate, Wire, Tube, Bar

Copper

0.03 %

Show Material materials with Copper of 0.03 %

F

EN 573-3, EN 1715-3, EN 485, EN 570, EN 755

Rod, Flat, Strip, Sheet, Plate, Wire, Tube, Bar

Iron

0.25 %

Show Material materials with Iron of 0.25 %

F

EN 573-3

Rod, Flat

0.25 %

Show Material materials with Iron of 0.25 %

F

EN 573-3, EN 1715-3, EN 485, EN 570, EN 755

Strip, Sheet, Plate, Wire, Tube, Bar

Magnesium

0.03 %

Show Material materials with Magnesium of 0.03 %

F

EN 573-3, EN 1715-3, EN 485, EN 570, EN 755

Rod, Flat, Strip, Sheet, Plate, Wire, Tube, Bar

Manganese

0.03 %

Show Material materials with Manganese of 0.03 %

F

EN 573-3, EN 1715-3, EN 485, EN 570, EN 755

Rod, Flat, Strip, Sheet, Plate, Wire, Tube, Bar

Silicon

0.2 %

Show Material materials with Silicon of 0.2 %

F

EN 573-3, EN 1715-3, EN 485, EN 570, EN 755

Rod, Flat, Strip, Sheet, Plate, Wire, Tube, Bar

Titanium

0.03 %

Show Material materials with Titanium of 0.03 %

F

EN 573-3, EN 1715-3, EN 485, EN 570, EN 755

Rod, Flat, Strip, Sheet, Plate, Wire, Tube, Bar

Zinc

0.07 %

Show Material materials with Zinc of 0.07 %

F

EN 573-3, EN 1715-3, EN 485, EN 570, EN 755

Rod, Flat, Strip, Sheet, Plate, Wire, Tube, Bar

Technological properties

Property
Anodizing

decorative: very good, Protective: very good

Brazing

hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good

Workability

Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H14) / very good (H12)