EN 573-3 Grade AW-1100 O

Want to keep this datasheet? Save it now in your required format

Description

EN AW-1100 is a soft, non-heat-treatable and low strength alloy that offers strong corrosion resistance. Composed of 99% aluminum and 0.12% copper, EN AW-1100 is purest grade of aluminum alloy available commercially.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey,Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated StandardsShape

Density

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

O

EN 573-3, EN 683

Strip, Sheet

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

O

EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209

Coil, Sheet, Foil

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

O

EN 573-3, EN 683

Strip, Sheet

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

O

EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209

Coil, Sheet, Foil

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 1000 Series Aluminium

Shear modulus

26.0 GPa

Show Material materials with Shear modulus of 26.0 GPa

O

EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209

Coil, Sheet, Foil

Tensile strength

20.0 °C

60.0 - 105.0 MPa

Show Material materials with Tensile strength of 60.0 - 105.0 MPa

O

EN 573-3, EN 683

Strip, Sheet, Foil

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

O

EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209

Coil, Sheet, Foil

20-100°C

100 °C, 20 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

O

EN 573-3, EN 683

Strip, Sheet

Melting point

640.0 - 655.0 °C

Show Material materials with Melting point of 640.0 - 655.0 °C

O

EN 573-3, EN 683

Strip, Sheet

Specific heat capacity

900.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 - 963.0 J/(kg·K)

Typical for Wrought 1000 Series Aluminium

Thermal conductivity

222.0 W/(m·K)

Show Material materials with Thermal conductivity of 222.0 W/(m·K)

O

EN 573-3, EN 683

Strip, Sheet

218.0 - 222.0 W/(m·K)

Show Material materials with Thermal conductivity of 218.0 - 222.0 W/(m·K)

O

EN 573-3, EN 683

Strip, Sheet

218 W/(m·K)

Show Material materials with Thermal conductivity of 218 W/(m·K)

O

EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209

Coil, Sheet, Foil

Electrical

PropertyValueConditionRelated StandardsShape

Electrical conductivity

34000000.0 S/m

Show Material materials with Electrical conductivity of 34000000.0 S/m

O

EN 573-3, EN 683

Strip, Sheet

33000000.0 - 34000000.0 S/m

Show Material materials with Electrical conductivity of 33000000.0 - 34000000.0 S/m

O

EN 573-3, EN 683

Strip, Sheet

Electrical resistivity

2.94e-08 Ω·m

Show Material materials with Electrical resistivity of 2.94e-08 Ω·m

O

EN 573-3, EN 683

Strip, Sheet

2.94e-08 - 3.03e-08 Ω·m

Show Material materials with Electrical resistivity of 2.94e-08 - 3.03e-08 Ω·m

O

EN 573-3, EN 683

Strip, Sheet

3.0000000000000004e-08 Ω·m

Show Material materials with Electrical resistivity of 3.0000000000000004e-08 Ω·m

O

EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209

Coil, Sheet, Foil

Chemical properties

PropertyValueConditionRelated StandardsShapeComment

Aluminium

99.0 %

Show Material materials with Aluminium of 99.0 %

O

EN 573-3, EN 683

Foil, Strip, Sheet

Copper

0.05 - 0.2 %

Show Material materials with Copper of 0.05 - 0.2 %

O

EN 573-3, EN 683, EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209

Foil, Strip, Sheet, Coil, Sheet, Foil

Iron

0.95 %

Show Material materials with Iron of 0.95 %

O

EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209

Coil, Sheet, Foil

Si + Fe

Manganese

0.05 %

Show Material materials with Manganese of 0.05 %

O

EN 573-3, EN 683

Foil, Strip, Sheet

0.05 %

Show Material materials with Manganese of 0.05 %

O

EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209

Coil, Sheet, Foil

Other

0.15 %

Show Material materials with Other of 0.15 %

O

EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209

Coil, Sheet, Foil

Silicon

0.95 %

Show Material materials with Silicon of 0.95 %

O

EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209

Coil, Sheet, Foil

Si + Fe

Zinc

0.1 %

Show Material materials with Zinc of 0.1 %

O

EN 573-3, EN 683

Foil, Strip, Sheet

0.1 %

Show Material materials with Zinc of 0.1 %

O

EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209

Coil, Sheet, Foil

Technological properties

Property
Anodizing

Very Good

Application areas

Roofing: Foil for bituminous coating; Interiors and ceilings: Decoration; Lighting: Anodizing Quality, Lacquering quality; Electronic devices: Housing of devices; Heat exchangers: Fins, General applications; Tubes: Industrial tubes, Flexible tube, Pipes; Insulation; Solar: Solar collectors; Wind energy: Nacelle coverings, Rotor, Hub, Stairs; Components: Automotive fins, Heat exchangers

Brazing

Excellent

Corrosion properties

Very Good

Welding

Excellent

Workability

Excellent