EN 573-3 Grade AW-1200 O

Want to keep this datasheet? Save it now in your required format

Description

Food safe aluminum.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey,Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.69 g/cm³

Show Material materials with Density of 2.69 g/cm³

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, EN 683-2

Coil, Sheet, Foil

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

O

EN 573-3

Sheet, Strip, Foil, Rod, Flat, Tube

20.0 °C

2.71 - 2.72 g/cm³

Show Material materials with Density of 2.71 - 2.72 g/cm³

O

EN 573-3

Sheet, Strip, Foil, Rod, Flat, Tube

20.0 °C

2.72 g/cm³

Show Material materials with Density of 2.72 g/cm³

O

EN 573-3

Sheet, Strip, Foil, Rod, Flat, Tube

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.2 mm

Show Material materials with Thickness of 0.2 mm

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2

0.2 mm

Coil, Sheet, Foil

3.0 mm

Show Material materials with Thickness of 3.0 mm

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2

3.0 mm

Coil, Sheet, Foil

40 mm

Show Material materials with Thickness of 40 mm

O

EN 546-2, EN 573-1, EN 573-2, EN 573-3, EN 485-2

40 mm

Coil, Sheet, Foil

60 mm

Show Material materials with Thickness of 60 mm

O

EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2

60 mm

Coil, Sheet, Foil

200 mm

Show Material materials with Thickness of 200 mm

O

EN 546-2, EN 573-1, EN 573-2, EN 573-3, EN 485-2

200 mm

Coil, Sheet, Foil

400 mm

Show Material materials with Thickness of 400 mm

O

EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2

400 mm

Coil, Sheet, Foil

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

35.0 MPa

Show Material materials with Bending Fatigue Strength of 35.0 MPa

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Bending angle 180°

0 °/t

Show Material materials with Bending angle 180° of 0 °/t

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2

Coil, Sheet, Foil

0.5 °/t

Show Material materials with Bending angle 180° of 0.5 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

1.0 °/t

Show Material materials with Bending angle 180° of 1.0 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Bending angle 90°

0 °/t

Show Material materials with Bending angle 90° of 0 °/t

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2

Coil, Sheet, Foil

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Elastic modulus

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, EN 683-2

Coil, Sheet, Foil

20.0 °C

60.0 - 65.0 GPa

Show Material materials with Elastic modulus of 60.0 - 65.0 GPa

O

EN 573-3

Sheet, Strip, Foil, Rod, Flat, Tube

20.0 °C

60.0 - 69.0 GPa

Show Material materials with Elastic modulus of 60.0 - 69.0 GPa

O

EN 573-3

Sheet, Strip, Foil, Rod, Flat, Tube

20.0 °C

65.0 - 69.0 GPa

Show Material materials with Elastic modulus of 65.0 - 69.0 GPa

O

EN 573-3

Sheet, Strip, Foil, Rod, Flat, Tube

20.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

O

EN 573-3

Sheet, Strip, Foil, Rod, Flat, Tube

Elongation

1.0 %

Show Material materials with Elongation of 1.0 %

O

EN 573-3, EN 546

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

3.0 %

Show Material materials with Elongation of 3.0 %

O

EN 573-3, EN 546

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

6.0 %

Show Material materials with Elongation of 6.0 %

O

EN 573-3, EN 546

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

6 %

Show Material materials with Elongation of 6 %

O

EN 546-2, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Foil

A50

10.0 %

Show Material materials with Elongation of 10.0 %

O

EN 573-3, EN 546, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

10 %

Show Material materials with Elongation of 10 %

O

EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2

Coil, Sheet, Foil

A50

14.0 %

Show Material materials with Elongation of 14.0 %

O

EN 573-3, EN 546, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

16.0 %

Show Material materials with Elongation of 16.0 %

O

EN 573-3, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

18.0 %

Show Material materials with Elongation of 18.0 %

O

EN 573-3, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

19.0 %

Show Material materials with Elongation of 19.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

19 %

Show Material materials with Elongation of 19 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2

Coil, Sheet, Foil

A50

20.0 %

Show Material materials with Elongation of 20.0 %

O

EN 573-3, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A100

20.0 %

Show Material materials with Elongation of 20.0 %

O

EN 573-3, EN 1396

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

21.0 %

Show Material materials with Elongation of 21.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

22.0 %

Show Material materials with Elongation of 22.0 %

O

EN 573-3, EN 1396

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

24.0 %

Show Material materials with Elongation of 24.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

26.0 %

Show Material materials with Elongation of 26.0 %

O

EN 573-3, EN 1396

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

28.0 %

Show Material materials with Elongation of 28.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

30.0 %

Show Material materials with Elongation of 30.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A100

33.0 %

Show Material materials with Elongation of 33.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

20.0 °C

1.0 %

Show Material materials with Elongation of 1.0 %

O

EN 573-3

Foil

A100

20.0 °C

1.0 %

Show Material materials with Elongation of 1.0 %

O

EN 573-3

Foil

A50

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

O

EN 573-3

Foil

A100

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

O

EN 573-3

Foil

A50

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

O

EN 573-3

Foil

A100

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

O

EN 573-3

Foil

A50

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

O

EN 573-3

Foil

A100

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

O

EN 573-3

Foil

A50

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

O

EN 573-3

Foil

A100

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

O

EN 573-3

Foil

A50

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

O

EN 573-3

Foil

A100

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

O

EN 573-3

Foil

A50

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

O

EN 573-3

Foil

A100

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

O

EN 573-3

Foil

A50

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

O

EN 573-3

Rod, Tube

A50

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

O

EN 573-3

Foil

A100

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

O

EN 573-3

Foil

A50

20.0 °C

19.0 %

Show Material materials with Elongation of 19.0 %

O

EN 573-3

Sheet, Strip, Flat

A50 Transverse

20.0 °C

19.0 %

Show Material materials with Elongation of 19.0 %

O

EN 573-3

Sheet, Strip, Flat

A50

20.0 °C

20.0 %

Show Material materials with Elongation of 20.0 %

O

EN 573-3

Rod, Tube

20.0 °C

21.0 %

Show Material materials with Elongation of 21.0 %

O

EN 573-3

Sheet, Strip, Flat

A50 Transverse

20.0 °C

21.0 %

Show Material materials with Elongation of 21.0 %

O

EN 573-3

Sheet, Strip, Flat

A50

20.0 °C

24.0 %

Show Material materials with Elongation of 24.0 %

O

EN 573-3

Sheet, Strip, Flat

A50 Transverse

20.0 °C

24.0 %

Show Material materials with Elongation of 24.0 %

O

EN 573-3

Sheet, Strip, Flat

A50

20.0 °C

28.0 %

Show Material materials with Elongation of 28.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

28.0 %

Show Material materials with Elongation of 28.0 %

O

EN 573-3

Flat

A50

20.0 °C

30.0 %

Show Material materials with Elongation of 30.0 %

O

EN 573-3

Flat

20.0 °C

30.0 %

Show Material materials with Elongation of 30.0 %

O

EN 573-3

Flat

Transverse

20.0 °C

33.0 %

Show Material materials with Elongation of 33.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

33.0 %

Show Material materials with Elongation of 33.0 %

O

EN 573-3

Flat

A50

20.0 °C

40.0 %

Show Material materials with Elongation of 40.0 %

O

EN 573-3

100.0 °C

45.0 %

Show Material materials with Elongation of 45.0 %

O

EN 573-3

150.0 °C

55.0 %

Show Material materials with Elongation of 55.0 %

O

EN 573-3

200.0 °C

65.0 %

Show Material materials with Elongation of 65.0 %

O

EN 573-3

260.0 °C

75.0 %

Show Material materials with Elongation of 75.0 %

O

EN 573-3

315.0 °C

80.0 %

Show Material materials with Elongation of 80.0 %

O

EN 573-3

370.0 °C

85.0 %

Show Material materials with Elongation of 85.0 %

O

EN 573-3

Hardness, Brinell

23.0 [-]

Show Material materials with Hardness, Brinell of 23.0 [-]

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

20.0 [-]

Show Material materials with Hardness, Brinell of 20.0 [-]

O

EN 573-3

Rod, Tube

20.0 °C

23.0 [-]

Show Material materials with Hardness, Brinell of 23.0 [-]

O

EN 573-3

Rod, Flat, Tube

Hardness, HBW

23 [-]

Show Material materials with Hardness, HBW of 23 [-]

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2

Coil, Sheet, Foil

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

O

EN 573-3

Sheet, Strip, Foil, Rod, Flat, Tube

Shear modulus

25.9 GPa

Show Material materials with Shear modulus of 25.9 GPa

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, EN 683-2

Coil, Sheet, Foil

20.0 °C

24.0 - 26.0 GPa

Show Material materials with Shear modulus of 24.0 - 26.0 GPa

O

EN 573-3

Sheet, Strip, Foil, Rod, Flat, Tube

20.0 °C

24.0 - 25.9 GPa

Show Material materials with Shear modulus of 24.0 - 25.9 GPa

O

EN 573-3

Sheet, Strip, Foil, Rod, Flat, Tube

20.0 °C

25.9 - 26.0 GPa

Show Material materials with Shear modulus of 25.9 - 26.0 GPa

O

EN 573-3

Sheet, Strip, Foil, Rod, Flat, Tube

20.0 °C

25.9 GPa

Show Material materials with Shear modulus of 25.9 GPa

O

EN 573-3

Sheet, Strip, Foil, Rod, Flat, Tube

Tensile strength

65.0 - 95.0 MPa

Show Material materials with Tensile strength of 65.0 - 95.0 MPa

O

EN 573-3, EN 1396

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

40.0 - 95.0 MPa

Show Material materials with Tensile strength of 40.0 - 95.0 MPa

O

EN 573-3, EN 546

Foil, Strip, Sheet, Plate, Bar, Rod, Tube

20.0 °C

40.0 - 100.0 MPa

Show Material materials with Tensile strength of 40.0 - 100.0 MPa

O

EN 573-3

Foil

20.0 °C

40.0 - 105.0 MPa

Show Material materials with Tensile strength of 40.0 - 105.0 MPa

O

EN 573-3

Foil

20.0 °C

45.0 - 95.0 MPa

Show Material materials with Tensile strength of 45.0 - 95.0 MPa

O

EN 573-3

Foil

20.0 °C

45.0 - 100.0 MPa

Show Material materials with Tensile strength of 45.0 - 100.0 MPa

O

EN 573-3, EN 546

Foil, Strip, Sheet, Plate, Bar, Rod, Tube

20.0 °C

45.0 - 105.0 MPa

Show Material materials with Tensile strength of 45.0 - 105.0 MPa

O

EN 573-3

Foil

20.0 °C

50.0 - 95.0 MPa

Show Material materials with Tensile strength of 50.0 - 95.0 MPa

O

EN 573-3

Foil

20.0 °C

50.0 - 100.0 MPa

Show Material materials with Tensile strength of 50.0 - 100.0 MPa

O

EN 573-3

Foil

20.0 °C

50.0 - 105.0 MPa

Show Material materials with Tensile strength of 50.0 - 105.0 MPa

O

EN 573-3, EN 546

Foil, Strip, Sheet, Plate, Bar, Rod, Tube

20.0 °C

55.0 - 95.0 MPa

Show Material materials with Tensile strength of 55.0 - 95.0 MPa

O

EN 573-3

Foil

20.0 °C

55.0 - 100.0 MPa

Show Material materials with Tensile strength of 55.0 - 100.0 MPa

O

EN 573-3

Foil

20.0 °C

55.0 - 105.0 MPa

Show Material materials with Tensile strength of 55.0 - 105.0 MPa

O

EN 573-3, EN 546, EN 546-2, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Foil, Strip, Sheet, Plate, Bar, Rod, Tube, Coil, Sheet, Foil

20.0 °C

60.0 - 95.0 MPa

Show Material materials with Tensile strength of 60.0 - 95.0 MPa

O

EN 573-3

Foil

20.0 °C

60.0 - 100.0 MPa

Show Material materials with Tensile strength of 60.0 - 100.0 MPa

O

EN 573-3

Foil

20.0 °C

60.0 - 105.0 MPa

Show Material materials with Tensile strength of 60.0 - 105.0 MPa

O

EN 573-3, EN 546, EN 683, EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2

Foil, Strip, Sheet, Plate, Bar, Rod, Tube, Coil, Sheet, Foil

20.0 °C

70.0 - 105.0 MPa

Show Material materials with Tensile strength of 70.0 - 105.0 MPa

O

EN 573-3, EN 754

Rod, Tube, Strip, Sheet, Plate, Foil, Bar

20.0 °C

75.0 - 105.0 MPa

Show Material materials with Tensile strength of 75.0 - 105.0 MPa

O

EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2

Sheet, Strip, Flat, Plate, Foil, Bar, Rod, Tube, Coil, Sheet, Foil

20.0 °C

75.0 - 105.0 MPa

Show Material materials with Tensile strength of 75.0 - 105.0 MPa

O

EN 573-3

Sheet, Strip, Flat

Transverse

20.0 °C

90.0 MPa

Show Material materials with Tensile strength of 90.0 MPa

O

EN 573-3

100.0 °C

70.0 MPa

Show Material materials with Tensile strength of 70.0 MPa

O

EN 573-3

150.0 °C

55.0 MPa

Show Material materials with Tensile strength of 55.0 MPa

O

EN 573-3

200.0 °C

40.0 MPa

Show Material materials with Tensile strength of 40.0 MPa

O

EN 573-3

260.0 °C

30.0 MPa

Show Material materials with Tensile strength of 30.0 MPa

O

EN 573-3

315.0 °C

20.0 MPa

Show Material materials with Tensile strength of 20.0 MPa

O

EN 573-3

370.0 °C

15.0 MPa

Show Material materials with Tensile strength of 15.0 MPa

O

EN 573-3

Yield strength

20.0 MPa

Show Material materials with Yield strength of 20.0 MPa

O

EN 573-3, EN 1396

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

RP02

25.0 MPa

Show Material materials with Yield strength of 25.0 MPa

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

RP02

25 MPa

Show Material materials with Yield strength of 25 MPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2

Coil, Sheet, Foil

65.0 MPa

Show Material materials with Yield strength of 65.0 MPa

O

EN 573-3, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

RP02

65 MPa

Show Material materials with Yield strength of 65 MPa

O

EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2

Coil, Sheet, Foil

20.0 °C

25.0 MPa

Show Material materials with Yield strength of 25.0 MPa

O

EN 573-3

Flat

RP02

20.0 °C

25.0 MPa

Show Material materials with Yield strength of 25.0 MPa

O

EN 573-3

Flat

RP02 Transverse

20.0 °C

30.0 MPa

Show Material materials with Yield strength of 30.0 MPa

O

EN 573-3

Sheet, Strip

RP02

20.0 °C

30.0 MPa

Show Material materials with Yield strength of 30.0 MPa

O

EN 573-3

Sheet, Strip

RP02 Transverse

20.0 °C

35.0 MPa

Show Material materials with Yield strength of 35.0 MPa

O

EN 573-3

RP02

20.0 °C

60.0 MPa

Show Material materials with Yield strength of 60.0 MPa

O

EN 573-3

Foil

RP02

20.0 °C

65.0 MPa

Show Material materials with Yield strength of 65.0 MPa

O

EN 573-3

Foil

RP02

100.0 °C

30.0 MPa

Show Material materials with Yield strength of 30.0 MPa

O

EN 573-3

Sheet, Strip

RP02

150.0 °C

30.0 MPa

Show Material materials with Yield strength of 30.0 MPa

O

EN 573-3

Sheet, Strip

RP02

200.0 °C

25.0 MPa

Show Material materials with Yield strength of 25.0 MPa

O

EN 573-3

Flat

RP02

260.0 °C

20.0 MPa

Show Material materials with Yield strength of 20.0 MPa

O

EN 573-3

RP02

315.0 °C

15.0 MPa

Show Material materials with Yield strength of 15.0 MPa

O

EN 573-3

RP02

370.0 °C

10.0 MPa

Show Material materials with Yield strength of 10.0 MPa

O

EN 573-3

RP02

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

-50 °C

2.17e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

-50.0 °C

2.17e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20 °C

2.17e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20 °C

2.4399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4399999999999997e-05 1/K

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20 °C

2.5399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5399999999999997e-05 1/K

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

100 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

100.0 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, EN 683-2

Coil, Sheet, Foil

20-100°C

200 °C

2.4399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4399999999999997e-05 1/K

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

200.0 °C

2.44e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.44e-05 1/K

O

EN 573-3

Sheet, Strip, Foil, Rod, Flat, Tube

300 °C

2.5399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5399999999999997e-05 1/K

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

300.0 °C

2.54e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.54e-05 1/K

O

EN 573-3

Sheet, Strip, Foil, Rod, Flat, Tube

Melting point

644.0 - 657.0 °C

Show Material materials with Melting point of 644.0 - 657.0 °C

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Specific heat capacity

20.0 °C

898.0 J/(kg·K)

Show Material materials with Specific heat capacity of 898.0 J/(kg·K)

O

EN 573-3

Sheet, Strip, Foil, Rod, Flat, Tube

Thermal conductivity

138 W/(m·K)

Show Material materials with Thermal conductivity of 138 W/(m·K)

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, EN 683-2

Coil, Sheet, Foil

20.0 °C

205.0 - 210.0 W/(m·K)

Show Material materials with Thermal conductivity of 205.0 - 210.0 W/(m·K)

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20.0 °C

205.0 - 225.0 W/(m·K)

Show Material materials with Thermal conductivity of 205.0 - 225.0 W/(m·K)

O

EN 573-3

Sheet, Strip, Foil, Rod, Flat, Tube

20.0 °C

210.0 - 225.0 W/(m·K)

Show Material materials with Thermal conductivity of 210.0 - 225.0 W/(m·K)

O

EN 573-3

Sheet, Strip, Foil, Rod, Flat, Tube

20.0 °C

225.0 W/(m·K)

Show Material materials with Thermal conductivity of 225.0 W/(m·K)

O

EN 573-3

Sheet, Strip, Foil, Rod, Flat, Tube

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

33000000.0 - 34000000.0 S/m

Show Material materials with Electrical conductivity of 33000000.0 - 34000000.0 S/m

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

34400000.0 - 35500000.0 S/m

Show Material materials with Electrical conductivity of 34400000.0 - 35500000.0 S/m

O

EN 573-3

Sheet, Strip, Foil, Rod, Flat, Tube

Electrical resistivity

2.94e-08 - 3.03e-08 Ω·m

Show Material materials with Electrical resistivity of 2.94e-08 - 3.03e-08 Ω·m

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

4.9e-08 Ω·m

Show Material materials with Electrical resistivity of 4.9e-08 Ω·m

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, EN 683-2

Coil, Sheet, Foil

20.0 °C

2.95e-08 Ω·m

Show Material materials with Electrical resistivity of 2.95e-08 Ω·m

O

EN 573-3

Sheet, Strip, Foil, Rod, Flat, Tube

Chemical properties

PropertyValueConditionRelated StandardsShapeComment

Aluminium

99.0 %

Show Material materials with Aluminium of 99.0 %

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754

Sheet, Strip, Foil, Rod, Flat, Tube, Plate, Bar

Copper

0.05 %

Show Material materials with Copper of 0.05 %

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754

Sheet, Strip, Foil, Rod, Flat, Tube, Plate, Bar

0.05 %

Show Material materials with Copper of 0.05 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, EN 683-2

Coil, Sheet, Foil

Iron

1 %

Show Material materials with Iron of 1 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, EN 683-2

Coil, Sheet, Foil

Si + Fe

Manganese

0.05 %

Show Material materials with Manganese of 0.05 %

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754

Sheet, Strip, Foil, Rod, Flat, Tube, Plate, Bar

0.05 %

Show Material materials with Manganese of 0.05 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, EN 683-2

Coil, Sheet, Foil

Other

0.15 %

Show Material materials with Other of 0.15 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, EN 683-2

Coil, Sheet, Foil

Silicon

1 %

Show Material materials with Silicon of 1 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, EN 683-2

Coil, Sheet, Foil

Si + Fe

Titanium

0.05 %

Show Material materials with Titanium of 0.05 %

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754

Sheet, Strip, Foil, Rod, Flat, Tube, Plate, Bar

0.05 %

Show Material materials with Titanium of 0.05 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, EN 683-2

Coil, Sheet, Foil

Zinc

0.1 %

Show Material materials with Zinc of 0.1 %

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754

Sheet, Strip, Foil, Rod, Flat, Tube, Plate, Bar

0.1 %

Show Material materials with Zinc of 0.1 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, EN 683-2

Coil, Sheet, Foil

Technological properties

Property
Anodizing

decorative: acceptable, Protective: very good

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels; Roofing: Foil for bituminous coating; Doors: Sheets for composites/ sandwich Panels; Electronic devices: Housing of devices; Heat exchangers: Fins; Cable wrapping: Electric cable wrapping; Insulation; Solar: Solar collectors; Semi-rigid and corrugated: Smooth wall

Brazing

hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good

Corrosion properties

Seawater: sufficient, weathering: acceptable

Welding

Excellent

Workability

Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H12) / very good (H12)