Description

EN AW-7075 is a high-strength alloy that offers good stress-corrosion cracking resistance. Known as a mainstay in the aerospace industry since it was introduced, Aluminum 7075 brings moderate toughness as well as an excellent strength-to-weight ratio. It is also important to note that at sub-zero temperatures Aluminum 7075 increases in strength.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.8 g/cm³

Show Material materials with Density of 2.8 g/cm³

H111

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

2.8 g/cm³

Show Material materials with Density of 2.8 g/cm³

H111

EN 573-3

Rod, Tube

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

72.0 GPa

Show Material materials with Elastic modulus of 72.0 GPa

H111

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

70.0 - 73.0 GPa

Show Material materials with Elastic modulus of 70.0 - 73.0 GPa

H111

EN 573-3

Rod, Tube

Elongation

8.0 %

Show Material materials with Elongation of 8.0 %

H111

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A50

10.0 %

Show Material materials with Elongation of 10.0 %

H111

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A100

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

H111

EN 573-3

Rod, Tube

A50

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

H111

EN 573-3

Rod, Tube

Hardness, Brinell

20.0 °C

60.0 [-]

Show Material materials with Hardness, Brinell of 60.0 [-]

H111

EN 573-3

Rod, Tube

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 7000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 7000 Series Aluminium

Shear modulus

27.1 GPa

Show Material materials with Shear modulus of 27.1 GPa

H111

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

25.0 - 27.0 GPa

Show Material materials with Shear modulus of 25.0 - 27.0 GPa

H111

EN 573-3

Rod, Tube

Tensile strength

275.0

Show Material materials with Tensile strength of 275.0

H111

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

275.0

Show Material materials with Tensile strength of 275.0

H111

EN 573-3

Rod, Tube

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

-50 °C

2.16e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.16e-05 1/K

H111

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Rod

-50.0 °C

2.16e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.16e-05 1/K

H111

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Rod

20 °C

2.16e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.16e-05 1/K

H111

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Rod

20 °C

2.3399999999999996e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K

H111

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20 °C

2.43e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.43e-05 1/K

H111

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Rod

20 °C

2.52e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.52e-05 1/K

H111

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Rod

100 °C

2.3399999999999996e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K

H111

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

100.0 °C

2.34e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.34e-05 1/K

H111

EN 573-3

Rod, Tube

200 °C

2.43e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.43e-05 1/K

H111

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Rod

200.0 °C

2.43e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.43e-05 1/K

H111

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Rod

300 °C

2.52e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.52e-05 1/K

H111

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Rod

300.0 °C

2.52e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.52e-05 1/K

H111

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Rod

Melting point

480.0 - 640.0 °C

Show Material materials with Melting point of 480.0 - 640.0 °C

H111

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Specific heat capacity

862.0 J/(kg·K)

Show Material materials with Specific heat capacity of 862.0 J/(kg·K)

H111

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

862.0 J/(kg·K)

Show Material materials with Specific heat capacity of 862.0 J/(kg·K)

H111

EN 573-3

Rod, Tube

Thermal conductivity

20.0 °C

130.0 - 160.0 W/(m·K)

Show Material materials with Thermal conductivity of 130.0 - 160.0 W/(m·K)

H111

EN 573-3, EN 754, EN 755

Rod, Tube, Strip, Sheet, Plate, Forging, Welded Tube, Bar

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

19000000.0 - 23000000.0 S/m

Show Material materials with Electrical conductivity of 19000000.0 - 23000000.0 S/m

H111

EN 573-3, EN 754, EN 755

Rod, Tube, Strip, Sheet, Plate, Forging, Welded Tube, Bar

Electrical resistivity

4.35e-08 - 5.26e-08 Ω·m

Show Material materials with Electrical resistivity of 4.35e-08 - 5.26e-08 Ω·m

H111

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.18 - 0.28 %

Show Material materials with Chromium of 0.18 - 0.28 %

H111

EN 573-3, EN 754, EN 755

Rod, Tube, Strip, Sheet, Plate, Forging, Welded Tube, Bar

Copper

1.2 - 2.0 %

Show Material materials with Copper of 1.2 - 2.0 %

H111

EN 573-3, EN 754, EN 755

Rod, Tube, Strip, Sheet, Plate, Forging, Welded Tube, Bar

Iron

0.5 %

Show Material materials with Iron of 0.5 %

H111

EN 573-3

Rod, Tube

0.50 %

Show Material materials with Iron of 0.50 %

H111

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Magnesium

2.1 - 2.9 %

Show Material materials with Magnesium of 2.1 - 2.9 %

H111

EN 573-3, EN 754, EN 755

Rod, Tube, Strip, Sheet, Plate, Forging, Welded Tube, Bar

Manganese

0.3 %

Show Material materials with Manganese of 0.3 %

H111

EN 573-3, EN 754, EN 755

Rod, Tube, Strip, Sheet, Plate, Forging, Welded Tube, Bar

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

H111

EN 573-3, EN 754, EN 755

Rod, Tube, Strip, Sheet, Plate, Forging, Welded Tube, Bar

Titanium

0.2 %

Show Material materials with Titanium of 0.2 %

H111

EN 573-3, EN 754, EN 755

Rod, Tube, Strip, Sheet, Plate, Forging, Welded Tube, Bar

Zinc

5.1 - 6.1 %

Show Material materials with Zinc of 5.1 - 6.1 %

H111

EN 573-3, EN 754, EN 755

Rod, Tube, Strip, Sheet, Plate, Forging, Welded Tube, Bar

Technological properties

Property
Anodizing

decorative: not suitable, Protective: acceptable

Brazing

hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: not suitable, soft brazing with flux: not suitable

Corrosion properties

Seawater: sufficient to poor, weathering: sufficient to poor

Workability