EN 573-3 Grade AW-1350 H12

Want to keep this datasheet? Save it now in your required format

Description

Excellent electrical conductivity.

Related Standards

Equivalent Materials

This material data has been provided by AluKey,Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated StandardsShape

Density

2.69 g/cm³

Show Material materials with Density of 2.69 g/cm³

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

2.705 g/cm³

Show Material materials with Density of 2.705 g/cm³

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.2 mm

Show Material materials with Thickness of 0.2 mm

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

0.2 mm

Coil, Sheet

3.0 mm

Show Material materials with Thickness of 3.0 mm

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

3.0 mm

Coil, Sheet

Mechanical

PropertyValueConditionRelated StandardsShapeComment

Bending angle 180°

0.5 °/t

Show Material materials with Bending angle 180° of 0.5 °/t

H12

EN 573-3, EN 485

Plate, Rod

1.0 °/t

Show Material materials with Bending angle 180° of 1.0 °/t

H12

EN 573-3, EN 485

Plate, Rod

Bending angle 90°

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

H12

EN 573-3, EN 485

Plate, Rod

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

H12

EN 573-3, EN 485

Plate, Rod

2.0 °/t

Show Material materials with Bending angle 90° of 2.0 °/t

H12

EN 573-3, EN 485

Plate, Rod

3 °/t

Show Material materials with Bending angle 90° of 3 °/t

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Elastic modulus

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Elongation

2.0 %

Show Material materials with Elongation of 2.0 %

H12

EN 573-3, EN 485

Plate, Rod

A50

4.0 %

Show Material materials with Elongation of 4.0 %

H12

EN 573-3, EN 485

Plate, Rod

A50

5.0 %

Show Material materials with Elongation of 5.0 %

H12

EN 573-3, EN 485

Plate, Rod

A50

7.0 %

Show Material materials with Elongation of 7.0 %

H12

EN 573-3, EN 485

Plate, Rod

A50

9.0 %

Show Material materials with Elongation of 9.0 %

H12

EN 573-3, EN 485

Plate, Rod

A50

9.0 %

Show Material materials with Elongation of 9.0 %

H12

EN 573-3, EN 485

Plate, Rod

20.0 %

Show Material materials with Elongation of 20.0 %

H12

EN 573-3, EN 1715-2

Plate, Rod

A50

Hardness, Brinell

28.0 [-]

Show Material materials with Hardness, Brinell of 28.0 [-]

H12

EN 573-3, EN 485

Plate, Rod

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 1000 Series Aluminium

Shear modulus

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Tensile strength

85.0 - 125.0 MPa

Show Material materials with Tensile strength of 85.0 - 125.0 MPa

H12

EN 573-3, EN 485

Plate, Rod

95.0 - 110.0 MPa

Show Material materials with Tensile strength of 95.0 - 110.0 MPa

H12

EN 573-3, EN 1715-2

Plate, Rod

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

20 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

100 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

100 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

20-100°C

Melting point

645.0 - 657.0 °C

Show Material materials with Melting point of 645.0 - 657.0 °C

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

645.0 - 655.0 °C

Show Material materials with Melting point of 645.0 - 655.0 °C

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

Specific heat capacity

900.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 - 963.0 J/(kg·K)

Typical for Wrought 1000 Series Aluminium

Thermal conductivity

138 W/(m·K)

Show Material materials with Thermal conductivity of 138 W/(m·K)

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

225.0 - 235.0 W/(m·K)

Show Material materials with Thermal conductivity of 225.0 - 235.0 W/(m·K)

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

234 W/(m·K)

Show Material materials with Thermal conductivity of 234 W/(m·K)

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

Electrical

PropertyValueConditionRelated StandardsShape

Electrical conductivity

35400000.0 - 36500000.0 S/m

Show Material materials with Electrical conductivity of 35400000.0 - 36500000.0 S/m

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

36000000.0 S/m

Show Material materials with Electrical conductivity of 36000000.0 S/m

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

Electrical resistivity

2.74e-08 - 2.82e-08 Ω·m

Show Material materials with Electrical resistivity of 2.74e-08 - 2.82e-08 Ω·m

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

2.78e-08 Ω·m

Show Material materials with Electrical resistivity of 2.78e-08 Ω·m

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

4.9e-08 Ω·m

Show Material materials with Electrical resistivity of 4.9e-08 Ω·m

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminium

99.5 %

Show Material materials with Aluminium of 99.5 %

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

Boron

0.05 %

Show Material materials with Boron of 0.05 %

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

Chromium

0.01 %

Show Material materials with Chromium of 0.01 %

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

0.01 %

Show Material materials with Chromium of 0.01 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Copper

0.05 %

Show Material materials with Copper of 0.05 %

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

0.05 %

Show Material materials with Copper of 0.05 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Gallium

0.03 %

Show Material materials with Gallium of 0.03 %

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

Iron

0.40 %

Show Material materials with Iron of 0.40 %

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

0.4 %

Show Material materials with Iron of 0.4 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Manganese

0.01 %

Show Material materials with Manganese of 0.01 %

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

0.01 %

Show Material materials with Manganese of 0.01 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Other

0.1 %

Show Material materials with Other of 0.1 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Silicon

0.1 %

Show Material materials with Silicon of 0.1 %

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

0.1 %

Show Material materials with Silicon of 0.1 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Zinc

0.05 %

Show Material materials with Zinc of 0.05 %

H12

EN 573-3, EN 1715-2, EN 485

Plate, Rod

0.05 %

Show Material materials with Zinc of 0.05 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Technological properties

Property
Anodizing

Good (For surface protection only)

Application areas

Conductors; rods for the manufacture of aluminium conductor wires.

Brazing

Excellent

Corrosion properties

Very Good

Welding

Very Good

Workability

Very Good