EN 573-3 Grade AW-2007 T4

Want to keep this datasheet? Save it now in your required format

Description

Age-hardenable AlCu alloy. The alloy is not food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.85 g/cm³

Show Material materials with Density of 2.85 g/cm³

T4

EN 573-3, EN 755

Rod, Tube

20.0 °C

2.85 g/cm³

Show Material materials with Density of 2.85 g/cm³

T4

EN 573-3

Profile, Rod, Tube

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

72.5 GPa

Show Material materials with Elastic modulus of 72.5 GPa

T4

EN 573-3, EN 755

Rod, Tube

Elongation

6.0 %

Show Material materials with Elongation of 6.0 %

T4

EN 573-3, EN 755

Rod, Tube

A50

7.0 %

Show Material materials with Elongation of 7.0 %

T4

EN 573-3, EN 755

Rod, Tube

A100

8.0 %

Show Material materials with Elongation of 8.0 %

T4

EN 573-3, EN 755

Rod, Tube

A100

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

T4

EN 573-3

Profile, Rod, Tube

A50

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

T4

EN 573-3

Rod

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T4

EN 573-3

Profile, Tube, Rod

Hardness, Brinell

20.0 °C

95.0 [-]

Show Material materials with Hardness, Brinell of 95.0 [-]

T4

EN 573-3

Profile, Rod, Tube

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 2000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 2000 Series Aluminium

Shear modulus

27.3 GPa

Show Material materials with Shear modulus of 27.3 GPa

T4

EN 573-3, EN 755

Rod, Tube

Tensile strength

330.0 MPa

Show Material materials with Tensile strength of 330.0 MPa

T4

EN 573-3, EN 755

Rod, Tube

340.0 MPa

Show Material materials with Tensile strength of 340.0 MPa

T4

EN 573-3, EN 755

Rod, Tube

370.0 MPa

Show Material materials with Tensile strength of 370.0 MPa

T4

EN 573-3, EN 755

Rod, Tube

20.0 °C

330.0 MPa

Show Material materials with Tensile strength of 330.0 MPa

T4

EN 573-3

Rod

20.0 °C

340.0 MPa

Show Material materials with Tensile strength of 340.0 MPa

T4

EN 573-3

Rod

20.0 °C

370.0 MPa

Show Material materials with Tensile strength of 370.0 MPa

T4

EN 573-3

Profile, Tube, Rod

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

20 °C

2.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K

T4

EN 573-3, EN 755

Rod, Tube

100 °C

2.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K

T4

EN 573-3, EN 755

Rod, Tube

100.0 °C

2.4e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4e-05 1/K

T4

EN 573-3

Profile, Rod, Tube

Melting point

507.0 - 650.0 °C

Show Material materials with Melting point of 507.0 - 650.0 °C

T4

EN 573-3, EN 755

Rod, Tube

Specific heat capacity

860.0 J/(kg·K)

Show Material materials with Specific heat capacity of 860.0 J/(kg·K)

T4

EN 573-3, EN 755

Rod, Tube

20.0 °C

860.0 J/(kg·K)

Show Material materials with Specific heat capacity of 860.0 J/(kg·K)

T4

EN 573-3

Profile, Rod, Tube

Thermal conductivity

130.0 - 160.0 W/(m·K)

Show Material materials with Thermal conductivity of 130.0 - 160.0 W/(m·K)

T4

EN 573-3, EN 755

Rod, Tube

20.0 °C

116.0 - 168.0 W/(m·K)

Show Material materials with Thermal conductivity of 116.0 - 168.0 W/(m·K)

T4

EN 573-3

Profile, Rod, Tube

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

18000000.0 - 22000000.0 S/m

Show Material materials with Electrical conductivity of 18000000.0 - 22000000.0 S/m

T4

EN 573-3, EN 755

Profile, Rod, Tube

Electrical resistivity

4.55e-08 - 5.56e-08 Ω·m

Show Material materials with Electrical resistivity of 4.55e-08 - 5.56e-08 Ω·m

T4

EN 573-3, EN 755

Rod, Tube

Chemical properties

PropertyValueConditionRelated StandardsShape

Bismuth

0.2 %

Show Material materials with Bismuth of 0.2 %

T4

EN 573-3, EN 755

Profile, Rod, Tube

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

T4

EN 573-3, EN 755

Profile, Rod, Tube

Copper

3.3 - 4.6 %

Show Material materials with Copper of 3.3 - 4.6 %

T4

EN 573-3, EN 755

Profile, Rod, Tube

Iron

0.8 %

Show Material materials with Iron of 0.8 %

T4

EN 573-3

Profile, Rod, Tube

0.80 %

Show Material materials with Iron of 0.80 %

T4

EN 573-3, EN 755

Rod, Tube

Lead

0.8 - 1.5 %

Show Material materials with Lead of 0.8 - 1.5 %

T4

EN 573-3, EN 755

Profile, Rod, Tube

Magnesium

0.4 - 1.8 %

Show Material materials with Magnesium of 0.4 - 1.8 %

T4

EN 573-3, EN 755

Profile, Rod, Tube

Manganese

0.5 - 1.0 %

Show Material materials with Manganese of 0.5 - 1.0 %

T4

EN 573-3, EN 755

Profile, Rod, Tube

Nickel

0.2 %

Show Material materials with Nickel of 0.2 %

T4

EN 573-3, EN 755

Profile, Rod, Tube

Silicon

0.8 %

Show Material materials with Silicon of 0.8 %

T4

EN 573-3, EN 755

Profile, Rod, Tube

Tin

0.2 %

Show Material materials with Tin of 0.2 %

T4

EN 573-3, EN 755

Profile, Rod, Tube

Titanium

0.2 %

Show Material materials with Titanium of 0.2 %

T4

EN 573-3, EN 755

Profile, Rod, Tube

Zinc

0.8 %

Show Material materials with Zinc of 0.8 %

T4

EN 573-3, EN 755

Profile, Rod, Tube

Technological properties

Property
Anodizing

Protective: poor

Brazing

friction soldering: sufficient

Corrosion properties

Seawater: poor, weathering: poor

Workability

Bending / Spinning (cold): sufficient / -, Deep drawing / upsetting (Condition) - / sufficient