Description

Aluminum EN AW-2011 is a popular age-hardenable alloy known for its free-machining characteristics and mechanical properties. It can be machined to very close tolerances while still maintaining a smooth and bright finish. Unlike other aluminum alloys, EN AW-2011 does not offer good corrosion resistance or weldability.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.82 g/cm³

Show Material materials with Density of 2.82 g/cm³

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar

2.83 g/cm³

Show Material materials with Density of 2.83 g/cm³

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar

20.0 °C

2.82 g/cm³

Show Material materials with Density of 2.82 g/cm³

T8

EN 573-3

Rod, Tube, Wire

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

125.0 MPa

Show Material materials with Bending Fatigue Strength of 125.0 MPa

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar

Elastic modulus

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar

72.5 GPa

Show Material materials with Elastic modulus of 72.5 GPa

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar

Elongation

4.0 %

Show Material materials with Elongation of 4.0 %

T8

EN 573-3, EN 1301

Strip, Sheet, Plate, Tube, Bar

6.0 %

Show Material materials with Elongation of 6.0 %

T8

EN 573-3, EN 754

Strip, Sheet, Plate, Tube, Bar

A50

8.0 %

Show Material materials with Elongation of 8.0 %

T8

EN 573-3, EN 754

Strip, Sheet, Plate, Tube, Bar

A100

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

T8

EN 573-3

Rod, Tube

A50

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

T8

EN 573-3

Wire

A100

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T8

EN 573-3

Rod, Tube

Hardness, Brinell

20.0 °C

115.0 [-]

Show Material materials with Hardness, Brinell of 115.0 [-]

T8

EN 573-3

Rod, Tube

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 2000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 2000 Series Aluminium

Shear modulus

27.3 GPa

Show Material materials with Shear modulus of 27.3 GPa

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar

Tensile strength

370.0 MPa

Show Material materials with Tensile strength of 370.0 MPa

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar

20.0 °C

310.0 MPa

Show Material materials with Tensile strength of 310.0 MPa

T8

EN 573-3

Wire

20.0 °C

370.0 MPa

Show Material materials with Tensile strength of 370.0 MPa

T8

EN 573-3

Rod, Tube

Unlock all property charts

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

-50 °C

2.14e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.14e-05 1/K

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar, Rod, Wire

-50.0 °C

2.14e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.14e-05 1/K

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar, Rod, Wire

20 °C

2.14e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.14e-05 1/K

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar, Rod, Wire

20 °C

2.2899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2899999999999998e-05 1/K

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar

20 °C

2.3399999999999996e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar

20 °C

2.4e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4e-05 1/K

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar, Rod, Wire

20 °C

2.4999999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4999999999999998e-05 1/K

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar

100 °C

2.2899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2899999999999998e-05 1/K

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar

100.0 °C

2.29e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.29e-05 1/K

T8

EN 573-3

Rod, Tube, Wire

100.0 °C

2.29e-05 - 2.31e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.29e-05 - 2.31e-05 1/K

T8

EN 573-3

Rod, Tube, Wire

100.0 °C

2.31e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.31e-05 1/K

T8

EN 573-3

Rod, Tube, Wire

100 °C

2.3399999999999996e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar

200 °C

2.4e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4e-05 1/K

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar, Rod, Wire

200.0 °C

2.4e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4e-05 1/K

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar, Rod, Wire

300 °C

2.4999999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4999999999999998e-05 1/K

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar

300.0 °C

2.5e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5e-05 1/K

T8

EN 573-3

Rod, Tube, Wire

Unlock all property charts

Melting point

540.0 - 645.0 °C

Show Material materials with Melting point of 540.0 - 645.0 °C

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar

585.0 - 650.0 °C

Show Material materials with Melting point of 585.0 - 650.0 °C

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar

Specific heat capacity

864.0 J/(kg·K)

Show Material materials with Specific heat capacity of 864.0 J/(kg·K)

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar

20.0 °C

864.0 J/(kg·K)

Show Material materials with Specific heat capacity of 864.0 J/(kg·K)

T8

EN 573-3

Rod, Tube, Wire

Thermal conductivity

170.0 - 220.0 W/(m·K)

Show Material materials with Thermal conductivity of 170.0 - 220.0 W/(m·K)

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar

20.0 °C

151.0 - 172.0 W/(m·K)

Show Material materials with Thermal conductivity of 151.0 - 172.0 W/(m·K)

T8

EN 573-3, EN 1301, EN 754

Rod, Tube, Wire, Strip, Sheet, Plate, Bar

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

24000000.0 - 32000000.0 S/m

Show Material materials with Electrical conductivity of 24000000.0 - 32000000.0 S/m

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar

20.0 °C

23000000.0 - 26000000.0 S/m

Show Material materials with Electrical conductivity of 23000000.0 - 26000000.0 S/m

T8

EN 573-3, EN 1301, EN 754

Rod, Tube, Wire, Strip, Sheet, Plate, Bar

Electrical resistivity

3.13e-08 - 4.17e-08 Ω·m

Show Material materials with Electrical resistivity of 3.13e-08 - 4.17e-08 Ω·m

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar

3.85e-08 - 4.35e-08 Ω·m

Show Material materials with Electrical resistivity of 3.85e-08 - 4.35e-08 Ω·m

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar

Chemical properties

PropertyValueConditionRelated StandardsShape

Bismuth

0.2 - 0.6 %

Show Material materials with Bismuth of 0.2 - 0.6 %

T8

EN 573-3, EN 1301, EN 754

Rod, Tube, Wire, Strip, Sheet, Plate, Bar

Copper

4.5 - 6.0 %

Show Material materials with Copper of 4.5 - 6.0 %

T8

EN 573-3

Rod, Tube

5.0 - 6.0 %

Show Material materials with Copper of 5.0 - 6.0 %

T8

EN 573-3, EN 1301, EN 754

Rod, Tube, Wire, Strip, Sheet, Plate, Bar

Iron

0.5 %

Show Material materials with Iron of 0.5 %

T8

EN 573-3

Rod, Tube

0.7 %

Show Material materials with Iron of 0.7 %

T8

EN 573-3

Rod, Tube, Wire

0.70 %

Show Material materials with Iron of 0.70 %

T8

EN 573-3, EN 1301, EN 754

Strip, Sheet, Plate, Tube, Bar

Lead

0.2 - 0.6 %

Show Material materials with Lead of 0.2 - 0.6 %

T8

EN 573-3, EN 1301, EN 754

Rod, Tube, Wire, Strip, Sheet, Plate, Bar

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

T8

EN 573-3, EN 1301, EN 754

Rod, Tube, Wire, Strip, Sheet, Plate, Bar

Zinc

0.3 %

Show Material materials with Zinc of 0.3 %

T8

EN 573-3, EN 1301, EN 754

Rod, Tube, Wire, Strip, Sheet, Plate, Bar

Technological properties

Property
Anodizing

decorative: not suitable, Protective: poor

Brazing

hard brazing (with flux/ without flux): not suitable /, friction soldering: sufficient

Corrosion properties

Seawater: poor, weathering: sufficient

Workability