EN 573-3 Grade AW-2011 F

Want to keep this datasheet? Save it now in your required format

Description

Aluminum EN AW-2011 is a popular age-hardenable alloy known for its free-machining characteristics and mechanical properties. It can be machined to very close tolerances while still maintaining a smooth and bright finish. Unlike other aluminum alloys, EN AW-2011 does not offer good corrosion resistance or weldability.

Related Standards

Equivalent Materials

This material data has been provided by AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated StandardsShape

Density

2.82 g/cm³

Show Material materials with Density of 2.82 g/cm³

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

2.83 g/cm³

Show Material materials with Density of 2.83 g/cm³

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Mechanical

PropertyValueConditionRelated StandardsShapeComment

Elastic modulus

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

72.5 GPa

Show Material materials with Elastic modulus of 72.5 GPa

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Hardness, Brinell

50.0 [-]

Show Material materials with Hardness, Brinell of 50.0 [-]

F

EN 573-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 2000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 2000 Series Aluminium

Shear modulus

27.3 GPa

Show Material materials with Shear modulus of 27.3 GPa

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Tensile strength

170.0 - 400.0 MPa

Show Material materials with Tensile strength of 170.0 - 400.0 MPa

F

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Tube, Bar

170.0 - 230.0 MPa

Show Material materials with Tensile strength of 170.0 - 230.0 MPa

F

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Tube, Bar

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

-50 °C

2.14e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.14e-05 1/K

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

20 °C

2.14e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.14e-05 1/K

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

20 °C

2.2899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2899999999999998e-05 1/K

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

20 °C

2.3399999999999996e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

20 °C

2.4e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4e-05 1/K

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

20 °C

2.4999999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4999999999999998e-05 1/K

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

100 °C

2.2899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2899999999999998e-05 1/K

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

100 °C

2.3399999999999996e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

200 °C

2.4e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4e-05 1/K

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

300 °C

2.4999999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4999999999999998e-05 1/K

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Melting point

540.0 - 645.0 °C

Show Material materials with Melting point of 540.0 - 645.0 °C

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

585.0 - 650.0 °C

Show Material materials with Melting point of 585.0 - 650.0 °C

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Specific heat capacity

864.0 J/(kg·K)

Show Material materials with Specific heat capacity of 864.0 J/(kg·K)

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Thermal conductivity

151.0 - 172.0 W/(m·K)

Show Material materials with Thermal conductivity of 151.0 - 172.0 W/(m·K)

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

170.0 - 220.0 W/(m·K)

Show Material materials with Thermal conductivity of 170.0 - 220.0 W/(m·K)

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Electrical

PropertyValueConditionRelated StandardsShape

Electrical conductivity

23000000.0 - 26000000.0 S/m

Show Material materials with Electrical conductivity of 23000000.0 - 26000000.0 S/m

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

24000000.0 - 32000000.0 S/m

Show Material materials with Electrical conductivity of 24000000.0 - 32000000.0 S/m

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Electrical resistivity

3.13e-08 - 4.17e-08 Ω·m

Show Material materials with Electrical resistivity of 3.13e-08 - 4.17e-08 Ω·m

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

3.85e-08 - 4.35e-08 Ω·m

Show Material materials with Electrical resistivity of 3.85e-08 - 4.35e-08 Ω·m

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Chemical properties

PropertyValueConditionRelated StandardsShape

Bismuth

0.2 - 0.6 %

Show Material materials with Bismuth of 0.2 - 0.6 %

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Copper

5.0 - 6.0 %

Show Material materials with Copper of 5.0 - 6.0 %

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Iron

0.70 %

Show Material materials with Iron of 0.70 %

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Lead

0.2 - 0.6 %

Show Material materials with Lead of 0.2 - 0.6 %

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Zinc

0.3 %

Show Material materials with Zinc of 0.3 %

F

EN 573-3, EN 1715-3, EN 570

Strip, Sheet, Plate, Tube, Bar

Technological properties

Property
Anodizing

decorative: not suitable, Protective: poor

Brazing

hard brazing (with flux/ without flux): not suitable /, friction soldering: sufficient

Corrosion properties

Seawater: poor, weathering: sufficient

Workability

Deep drawing / upsetting (Condition) - / acceptable