EN 573-3 Grade AW-2011 T4

Want to keep this datasheet? Save it now in your required format

Description

Aluminum EN AW-2011 is a popular age-hardenable alloy known for its free-machining characteristics and mechanical properties. It can be machined to very close tolerances while still maintaining a smooth and bright finish. Unlike other aluminum alloys, EN AW-2011 does not offer good corrosion resistance or weldability.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.82 g/cm³

Show Material materials with Density of 2.82 g/cm³

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

2.83 g/cm³

Show Material materials with Density of 2.83 g/cm³

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

20.0 °C

2.82 g/cm³

Show Material materials with Density of 2.82 g/cm³

T4

EN 573-3

Rod

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

125.0 MPa

Show Material materials with Bending Fatigue Strength of 125.0 MPa

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

Elastic modulus

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

72.5 GPa

Show Material materials with Elastic modulus of 72.5 GPa

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

Elongation

12.0 %

Show Material materials with Elongation of 12.0 %

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

A50

14.0 %

Show Material materials with Elongation of 14.0 %

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

A100

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

T4

EN 573-3

Rod

A50

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

T4

EN 573-3

Rod

Hardness, Brinell

20.0 °C

95.0 [-]

Show Material materials with Hardness, Brinell of 95.0 [-]

T4

EN 573-3

Rod

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 2000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 2000 Series Aluminium

Shear modulus

27.3 GPa

Show Material materials with Shear modulus of 27.3 GPa

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

Tensile strength

275.0 MPa

Show Material materials with Tensile strength of 275.0 MPa

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

20.0 °C

275.0 MPa

Show Material materials with Tensile strength of 275.0 MPa

T4

EN 573-3

Rod

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

-50 °C

2.14e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.14e-05 1/K

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar, Rod

-50.0 °C

2.14e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.14e-05 1/K

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar, Rod

20 °C

2.14e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.14e-05 1/K

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar, Rod

20 °C

2.2899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2899999999999998e-05 1/K

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

20 °C

2.3399999999999996e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

20 °C

2.4e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4e-05 1/K

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar, Rod

20 °C

2.4999999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4999999999999998e-05 1/K

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

100 °C

2.2899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2899999999999998e-05 1/K

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

100.0 °C

2.29e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.29e-05 1/K

T4

EN 573-3

Rod

100.0 °C

2.29e-05 - 2.31e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.29e-05 - 2.31e-05 1/K

T4

EN 573-3

Rod

100.0 °C

2.31e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.31e-05 1/K

T4

EN 573-3

Rod

100 °C

2.3399999999999996e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

200 °C

2.4e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4e-05 1/K

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar, Rod

200.0 °C

2.4e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4e-05 1/K

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar, Rod

300 °C

2.4999999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4999999999999998e-05 1/K

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

300.0 °C

2.5e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5e-05 1/K

T4

EN 573-3

Rod

Melting point

540.0 - 645.0 °C

Show Material materials with Melting point of 540.0 - 645.0 °C

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

585.0 - 650.0 °C

Show Material materials with Melting point of 585.0 - 650.0 °C

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

Specific heat capacity

864.0 J/(kg·K)

Show Material materials with Specific heat capacity of 864.0 J/(kg·K)

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

20.0 °C

864.0 J/(kg·K)

Show Material materials with Specific heat capacity of 864.0 J/(kg·K)

T4

EN 573-3

Rod

Thermal conductivity

170.0 - 220.0 W/(m·K)

Show Material materials with Thermal conductivity of 170.0 - 220.0 W/(m·K)

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

20.0 °C

151.0 - 172.0 W/(m·K)

Show Material materials with Thermal conductivity of 151.0 - 172.0 W/(m·K)

T4

EN 573-3, EN 755

Rod, Strip, Sheet, Plate, Tube, Bar

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

24000000.0 - 32000000.0 S/m

Show Material materials with Electrical conductivity of 24000000.0 - 32000000.0 S/m

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

20.0 °C

23000000.0 - 26000000.0 S/m

Show Material materials with Electrical conductivity of 23000000.0 - 26000000.0 S/m

T4

EN 573-3, EN 755

Rod, Strip, Sheet, Plate, Tube, Bar

Electrical resistivity

3.13e-08 - 4.17e-08 Ω·m

Show Material materials with Electrical resistivity of 3.13e-08 - 4.17e-08 Ω·m

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

3.85e-08 - 4.35e-08 Ω·m

Show Material materials with Electrical resistivity of 3.85e-08 - 4.35e-08 Ω·m

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

Chemical properties

PropertyValueConditionRelated StandardsShape

Bismuth

0.2 - 0.6 %

Show Material materials with Bismuth of 0.2 - 0.6 %

T4

EN 573-3, EN 755

Rod, Strip, Sheet, Plate, Tube, Bar

Copper

4.5 - 6.0 %

Show Material materials with Copper of 4.5 - 6.0 %

T4

EN 573-3

Rod

5.0 - 6.0 %

Show Material materials with Copper of 5.0 - 6.0 %

T4

EN 573-3, EN 755

Rod, Strip, Sheet, Plate, Tube, Bar

Iron

0.5 %

Show Material materials with Iron of 0.5 %

T4

EN 573-3

Rod

0.7 %

Show Material materials with Iron of 0.7 %

T4

EN 573-3

Rod

0.70 %

Show Material materials with Iron of 0.70 %

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

Lead

0.2 - 0.6 %

Show Material materials with Lead of 0.2 - 0.6 %

T4

EN 573-3, EN 755

Rod, Strip, Sheet, Plate, Tube, Bar

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

T4

EN 573-3, EN 755

Rod, Strip, Sheet, Plate, Tube, Bar

Zinc

0.3 %

Show Material materials with Zinc of 0.3 %

T4

EN 573-3, EN 755

Rod, Strip, Sheet, Plate, Tube, Bar

Technological properties

Property
Anodizing

decorative: not suitable, Protective: poor

Brazing

hard brazing (with flux/ without flux): not suitable /, friction soldering: sufficient

Corrosion properties

Seawater: poor, weathering: sufficient

Workability

Deep drawing / upsetting (Condition) - / acceptable