General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Density | 2.8 g/cm³ Show Material materials with Density of 2.8 g/cm³ | T4511 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 73.0 GPa Show Material materials with Elastic modulus of 73.0 GPa | T4511 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
Elongation | 8.0 % Show Material materials with Elongation of 8.0 % | T4511 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | |
8.0 % Show Material materials with Elongation of 8.0 % | T4511 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A100 | ||
10.0 % Show Material materials with Elongation of 10.0 % | T4511 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
10.0 % Show Material materials with Elongation of 10.0 % | T4511 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A100 | ||
11.0 % Show Material materials with Elongation of 11.0 % | T4511 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
11.0 % Show Material materials with Elongation of 11.0 % | T4511 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A100 | ||
12.0 % Show Material materials with Elongation of 12.0 % | T4511 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A100 | ||
13.0 % Show Material materials with Elongation of 13.0 % | T4511 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A100 | ||
20.0 °C | 8.0 % Show Material materials with Elongation of 8.0 % | T4511 | EN 573-3 | Tube | A50 | |
20.0 °C | 8.0 % Show Material materials with Elongation of 8.0 % | T4511 | EN 573-3 | Rod | ||
20.0 °C | 10.0 % Show Material materials with Elongation of 10.0 % | T4511 | EN 573-3 | Tube, Profile | A50 | |
20.0 °C | 10.0 % Show Material materials with Elongation of 10.0 % | T4511 | EN 573-3 | Tube, Profile, Rod | ||
20.0 °C | 11.0 % Show Material materials with Elongation of 11.0 % | T4511 | EN 573-3 | Rod | A50 | |
20.0 °C | 11.0 % Show Material materials with Elongation of 11.0 % | T4511 | EN 573-3 | Tube, Profile | ||
20.0 °C | 12.0 % Show Material materials with Elongation of 12.0 % | T4511 | EN 573-3 | Rod | ||
20.0 °C | 13.0 % Show Material materials with Elongation of 13.0 % | T4511 | EN 573-3 | Rod | ||
Hardness, Brinell | 20.0 °C | 110.0 [-] Show Material materials with Hardness, Brinell of 110.0 [-] | T4511 | EN 573-3 | Profile, Rod, Tube | |
20.0 °C | 110.0 - 140.0 [-] Show Material materials with Hardness, Brinell of 110.0 - 140.0 [-] | T4511 | EN 573-3 | Rod | ||
20.0 °C | 140.0 [-] Show Material materials with Hardness, Brinell of 140.0 [-] | T4511 | EN 573-3 | Rod | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Shear modulus | 27.4 GPa Show Material materials with Shear modulus of 27.4 GPa | T4511 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
Tensile strength | 350.0 MPa Show Material materials with Tensile strength of 350.0 MPa | T4511 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
370.0 MPa Show Material materials with Tensile strength of 370.0 MPa | T4511 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
380.0 MPa Show Material materials with Tensile strength of 380.0 MPa | T4511 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
390.0 MPa Show Material materials with Tensile strength of 390.0 MPa | T4511 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
410.0 MPa Show Material materials with Tensile strength of 410.0 MPa | T4511 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
20.0 °C | 350.0 MPa Show Material materials with Tensile strength of 350.0 MPa | T4511 | EN 573-3 | Rod | ||
20.0 °C | 370.0 MPa Show Material materials with Tensile strength of 370.0 MPa | T4511 | EN 573-3 | Tube, Profile, Rod | ||
20.0 °C | 380.0 MPa Show Material materials with Tensile strength of 380.0 MPa | T4511 | EN 573-3 | Tube | ||
20.0 °C | 390.0 MPa Show Material materials with Tensile strength of 390.0 MPa | T4511 | EN 573-3 | Rod | ||
20.0 °C | 410.0 MPa Show Material materials with Tensile strength of 410.0 MPa | T4511 | EN 573-3 | Profile, Rod |
Thermal
Property | Value | Comment |
---|---|---|
Coefficient of thermal expansion | 1.6e-05 - 2.4e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.6e-05 - 2.4e-05 1/K | Typical for Wrought 2000 Series Aluminium |
Melting point | 500.0 - 650.0 °C Show Material materials with Melting point of 500.0 - 650.0 °C | Typical for Wrought 2000 Series Aluminium |
Specific heat capacity | 816.0 - 963.0 J/(kg·K) Show Material materials with Specific heat capacity of 816.0 - 963.0 J/(kg·K) | Typical for Wrought 2000 Series Aluminium |
Thermal conductivity | 112.0 - 251.0 W/(m·K) Show Material materials with Thermal conductivity of 112.0 - 251.0 W/(m·K) | Typical for Wrought 2000 Series Aluminium |
Electrical
Property | Value | Comment |
---|---|---|
Electrical conductivity | 18000000.0 - 30000000.0 S/m Show Material materials with Electrical conductivity of 18000000.0 - 30000000.0 S/m | Typical for Wrought 2000 Series Aluminium |
Electrical resistivity | 3.4e-08 - 6e-08 Ω·m Show Material materials with Electrical resistivity of 3.4e-08 - 6e-08 Ω·m | Typical for Wrought 2000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Beryllium | 0.0001 - 0.005 % Show Material materials with Beryllium of 0.0001 - 0.005 % | T4511 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire |
Chromium | 0.1 % Show Material materials with Chromium of 0.1 % | T4511 | EN 573-3, EN 754, EN 755 | Tube, Profile, Rod, Strip, Sheet, Plate, Welded Tube, Wire |
Copper | 3.9 - 5.0 % Show Material materials with Copper of 3.9 - 5.0 % | T4511 | EN 573-3, EN 754, EN 755 | Tube, Profile, Rod, Strip, Sheet, Plate, Welded Tube, Wire |
Iron | 0.5 % Show Material materials with Iron of 0.5 % | T4511 | EN 573-3 | Tube, Profile, Rod |
0.50 % Show Material materials with Iron of 0.50 % | T4511 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |
Magnesium | 0.2 - 0.8 % Show Material materials with Magnesium of 0.2 - 0.8 % | T4511 | EN 573-3, EN 754, EN 755 | Tube, Profile, Rod, Strip, Sheet, Plate, Welded Tube, Wire |
Manganese | 0.4 - 1.2 % Show Material materials with Manganese of 0.4 - 1.2 % | T4511 | EN 573-3, EN 754, EN 755 | Tube, Profile, Rod, Strip, Sheet, Plate, Welded Tube, Wire |
Nickel | 0.1 % Show Material materials with Nickel of 0.1 % | T4511 | EN 573-3, EN 754, EN 755 | Tube, Profile, Rod, Strip, Sheet, Plate, Welded Tube, Wire |
Silicon | 0.5 - 0.9 % Show Material materials with Silicon of 0.5 - 0.9 % | T4511 | EN 573-3, EN 754, EN 755 | Tube, Profile, Rod, Strip, Sheet, Plate, Welded Tube, Wire |
Titanium | 0.15 % Show Material materials with Titanium of 0.15 % | T4511 | EN 573-3, EN 754, EN 755 | Tube, Profile, Rod, Strip, Sheet, Plate, Welded Tube, Wire |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | T4511 | EN 573-3, EN 754, EN 755 | Tube, Profile, Rod, Strip, Sheet, Plate, Welded Tube, Wire |
Technological properties
Property | ||
---|---|---|
Workability | Moderate Workability |