EN 573-3 Grade AW-2014 T4

Want to keep this datasheet? Save it now in your required format

Description

EN AW-2014 is an alloy with strength, machinability and welding capabilities, Aluminum Alloy EN AW-2014 is an excellent option. It is a precipitation hardening alloy that maintains strength after heat treatment.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.8 g/cm³

Show Material materials with Density of 2.8 g/cm³

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

20.0 °C

2.8 g/cm³

Show Material materials with Density of 2.8 g/cm³

T4

EN 573-3

Profile, Forging, Rod, Flat, Tube, Sheet

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

140.0 MPa

Show Material materials with Bending Fatigue Strength of 140.0 MPa

T4

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

Bending angle 180°

3.0 °/t

Show Material materials with Bending angle 180° of 3.0 °/t

T4

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

5.0 °/t

Show Material materials with Bending angle 180° of 5.0 °/t

T4

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

Bending angle 90°

3.0 °/t

Show Material materials with Bending angle 90° of 3.0 °/t

T4

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

5.0 °/t

Show Material materials with Bending angle 90° of 5.0 °/t

T4

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

8.0 °/t

Show Material materials with Bending angle 90° of 8.0 °/t

T4

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

Elastic modulus

73.0 GPa

Show Material materials with Elastic modulus of 73.0 GPa

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

20.0 °C

72.0 GPa

Show Material materials with Elastic modulus of 72.0 GPa

T4

EN 573-3

Profile, Forging, Rod, Flat, Tube, Sheet

Elongation

8.0 %

Show Material materials with Elongation of 8.0 %

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

A100

10.0 %

Show Material materials with Elongation of 10.0 %

T4

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

A50

10.0 %

Show Material materials with Elongation of 10.0 %

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

A100

11.0 %

Show Material materials with Elongation of 11.0 %

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

A50

11.0 %

Show Material materials with Elongation of 11.0 %

T4

EN 573-3, EN 586, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

A100

12.0 %

Show Material materials with Elongation of 12.0 %

T4

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

A100

13.0 %

Show Material materials with Elongation of 13.0 %

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

A100

14.0 %

Show Material materials with Elongation of 14.0 %

T4

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

A50

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

T4

EN 573-3

Sheet, Flat

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

T4

EN 573-3

Flat

Transverse

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T4

EN 573-3

Rod

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

T4

EN 573-3

Profile, Rod, Tube

A50

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

T4

EN 573-3

Flat, Profile, Rod

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

T4

EN 573-3

Flat

Transverse

20.0 °C

11.0 %

Show Material materials with Elongation of 11.0 %

T4

EN 573-3

Rod

A50

20.0 °C

11.0 %

Show Material materials with Elongation of 11.0 %

T4

EN 573-3

Forging, Tube, Profile

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

T4

EN 573-3

Rod, Tube, Flat

20.0 °C

13.0 %

Show Material materials with Elongation of 13.0 %

T4

EN 573-3

Flat

A50

20.0 °C

13.0 %

Show Material materials with Elongation of 13.0 %

T4

EN 573-3

Rod

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

T4

EN 573-3

Flat

A50

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

T4

EN 573-3

Flat

A50 Transverse

Hardness, Brinell

100.0 [-]

Show Material materials with Hardness, Brinell of 100.0 [-]

T4

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

110.0 [-]

Show Material materials with Hardness, Brinell of 110.0 [-]

T4

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

112.0 [-]

Show Material materials with Hardness, Brinell of 112.0 [-]

T4

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

20.0 °C

100.0 [-]

Show Material materials with Hardness, Brinell of 100.0 [-]

T4

EN 573-3

Forging

20.0 °C

110.0 [-]

Show Material materials with Hardness, Brinell of 110.0 [-]

T4

EN 573-3

Profile, Rod, Tube, Flat

20.0 °C

110.0 - 112.0 [-]

Show Material materials with Hardness, Brinell of 110.0 - 112.0 [-]

T4

EN 573-3

Flat

20.0 °C

110.0 - 111.0 [-]

Show Material materials with Hardness, Brinell of 110.0 - 111.0 [-]

T4

EN 573-3

Flat

20.0 °C

111.0 [-]

Show Material materials with Hardness, Brinell of 111.0 [-]

T4

EN 573-3

Sheet, Flat

20.0 °C

111.0 - 112.0 [-]

Show Material materials with Hardness, Brinell of 111.0 - 112.0 [-]

T4

EN 573-3

Flat

20.0 °C

112.0 [-]

Show Material materials with Hardness, Brinell of 112.0 [-]

T4

EN 573-3

Flat

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 2000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 2000 Series Aluminium

Shear modulus

27.4 GPa

Show Material materials with Shear modulus of 27.4 GPa

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

Tensile strength

350.0 MPa

Show Material materials with Tensile strength of 350.0 MPa

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

370.0 MPa

Show Material materials with Tensile strength of 370.0 MPa

T4

EN 573-3, EN 586, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

380.0 MPa

Show Material materials with Tensile strength of 380.0 MPa

T4

EN 573-3, EN 754

Strip, Sheet, Plate, Forging, Tube, Bar

390.0 MPa

Show Material materials with Tensile strength of 390.0 MPa

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

395.0 MPa

Show Material materials with Tensile strength of 395.0 MPa

T4

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

400.0 MPa

Show Material materials with Tensile strength of 400.0 MPa

T4

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

410.0 MPa

Show Material materials with Tensile strength of 410.0 MPa

T4

EN 573-3, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

20.0 °C

350.0 MPa

Show Material materials with Tensile strength of 350.0 MPa

T4

EN 573-3

Rod

20.0 °C

370.0 MPa

Show Material materials with Tensile strength of 370.0 MPa

T4

EN 573-3

Forging, Rod, Tube, Profile

20.0 °C

380.0 MPa

Show Material materials with Tensile strength of 380.0 MPa

T4

EN 573-3

Rod, Tube

20.0 °C

390.0 MPa

Show Material materials with Tensile strength of 390.0 MPa

T4

EN 573-3

Rod

20.0 °C

395.0 MPa

Show Material materials with Tensile strength of 395.0 MPa

T4

EN 573-3

Sheet, Flat

20.0 °C

395.0 MPa

Show Material materials with Tensile strength of 395.0 MPa

T4

EN 573-3

Flat

Transverse

20.0 °C

400.0 MPa

Show Material materials with Tensile strength of 400.0 MPa

T4

EN 573-3

Flat

20.0 °C

400.0 MPa

Show Material materials with Tensile strength of 400.0 MPa

T4

EN 573-3

Flat

Transverse

20.0 °C

410.0 MPa

Show Material materials with Tensile strength of 410.0 MPa

T4

EN 573-3

Rod, Profile

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

-50 °C

2.1e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

-50.0 °C

2.1e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

20 °C

2.1e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

20 °C

2.28e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.28e-05 1/K

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

20 °C

2.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

20 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

20 °C

2.46e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.46e-05 1/K

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

100 °C

2.28e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.28e-05 1/K

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

100.0 °C

2.28e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.28e-05 1/K

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

100 °C

2.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

200 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

200.0 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

300 °C

2.46e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.46e-05 1/K

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

300.0 °C

2.46e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.46e-05 1/K

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

Melting point

505.0 - 635.0 °C

Show Material materials with Melting point of 505.0 - 635.0 °C

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

510.0 - 640.0 °C

Show Material materials with Melting point of 510.0 - 640.0 °C

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

Specific heat capacity

816.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 816.0 - 963.0 J/(kg·K)

Typical for Wrought 2000 Series Aluminium

Thermal conductivity

134.0 - 193.0 W/(m·K)

Show Material materials with Thermal conductivity of 134.0 - 193.0 W/(m·K)

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

20.0 °C

140.0 - 200.0 W/(m·K)

Show Material materials with Thermal conductivity of 140.0 - 200.0 W/(m·K)

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Profile, Forging, Rod, Flat, Tube, Sheet, Strip, Plate, Bar

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

21000000.0 - 24000000.0 S/m

Show Material materials with Electrical conductivity of 21000000.0 - 24000000.0 S/m

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

20.0 °C

17000000.0 - 21000000.0 S/m

Show Material materials with Electrical conductivity of 17000000.0 - 21000000.0 S/m

T4

EN 573-3

Forging

20.0 °C

20000000.0 - 29000000.0 S/m

Show Material materials with Electrical conductivity of 20000000.0 - 29000000.0 S/m

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Forging, Bar

Electrical resistivity

3.45e-08 - 5e-08 Ω·m

Show Material materials with Electrical resistivity of 3.45e-08 - 5e-08 Ω·m

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

4.17e-08 - 4.76e-08 Ω·m

Show Material materials with Electrical resistivity of 4.17e-08 - 4.76e-08 Ω·m

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Profile, Forging, Rod, Flat, Tube, Sheet, Strip, Plate, Bar

Copper

3.9 - 5.0 %

Show Material materials with Copper of 3.9 - 5.0 %

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Profile, Forging, Rod, Flat, Tube, Sheet, Strip, Plate, Bar

Iron

0.5 %

Show Material materials with Iron of 0.5 %

T4

EN 573-3

Profile, Rod, Flat, Tube

0.7 %

Show Material materials with Iron of 0.7 %

T4

EN 573-3

Profile, Forging, Rod, Flat, Tube, Sheet

0.70 %

Show Material materials with Iron of 0.70 %

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

Magnesium

0.2 - 0.8 %

Show Material materials with Magnesium of 0.2 - 0.8 %

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Profile, Forging, Rod, Flat, Tube, Sheet, Strip, Plate, Bar

Manganese

0.4 - 1.2 %

Show Material materials with Manganese of 0.4 - 1.2 %

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Profile, Forging, Rod, Flat, Tube, Sheet, Strip, Plate, Bar

Nickel

0.1

Show Material materials with Nickel of 0.1

T4

EN 573-3

Profile, Rod, Flat, Tube

Silicon

0.5 - 1.2 %

Show Material materials with Silicon of 0.5 - 1.2 %

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Profile, Forging, Rod, Flat, Tube, Sheet, Strip, Plate, Bar

0.5 - 0.9 %

Show Material materials with Silicon of 0.5 - 0.9 %

T4

EN 573-3

Profile, Rod, Flat, Tube

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Profile, Forging, Rod, Flat, Tube, Sheet, Strip, Plate, Bar

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

T4

EN 573-3, EN 485, EN 586, EN 754, EN 755

Profile, Forging, Rod, Flat, Tube, Sheet, Strip, Plate, Bar

Technological properties

Property
Anodizing

decorative: not suitable, Protective: acceptable

Brazing

hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable

Corrosion properties

Seawater: sufficient, weathering: acceptable

Workability

Bending / Spinning (cold): gut (O) / ungeeignet, Impact extrusion (cold): not suitable, Deep drawing / upsetting (Condition) acceptable (O) / not suitable