General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 2.8 g/cm³ Show Material materials with Density of 2.8 g/cm³ | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |
20.0 °C | 2.8 g/cm³ Show Material materials with Density of 2.8 g/cm³ | T6 | EN 573-3 | Forging, Profile, Rod, Flat, Tube, Sheet |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 145.0 MPa Show Material materials with Bending Fatigue Strength of 145.0 MPa | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
Bending angle 90° | 5.0 °/t Show Material materials with Bending angle 90° of 5.0 °/t | T6 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
7.0 °/t Show Material materials with Bending angle 90° of 7.0 °/t | T6 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
10.0 °/t Show Material materials with Bending angle 90° of 10.0 °/t | T6 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
Elastic modulus | -269.0 °C | 82.2 GPa Show Material materials with Elastic modulus of 82.2 GPa | T6 | EN 573-3 | ||
-195.0 °C | 81.8 GPa Show Material materials with Elastic modulus of 81.8 GPa | T6 | EN 573-3 | |||
73.0 GPa Show Material materials with Elastic modulus of 73.0 GPa | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
20.0 °C | 72.0 GPa Show Material materials with Elastic modulus of 72.0 GPa | T6 | EN 573-3 | Forging, Profile, Rod, Flat, Tube, Sheet | ||
27.0 °C | 74.4 GPa Show Material materials with Elastic modulus of 74.4 GPa | T6 | EN 573-3 | |||
Elongation | 2.0 % Show Material materials with Elongation of 2.0 % | T6 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | A100 | |
3.0 % Show Material materials with Elongation of 3.0 % | T6 | EN 573-3, EN 586 | Strip, Sheet, Plate, Forging, Tube, Bar | A100 | ||
4.0 % Show Material materials with Elongation of 4.0 % | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | A50 | ||
4.0 % Show Material materials with Elongation of 4.0 % | T6 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | A100 | ||
5.0 % Show Material materials with Elongation of 5.0 % | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | A50 | ||
5.0 % Show Material materials with Elongation of 5.0 % | T6 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | A100 | ||
6.0 % Show Material materials with Elongation of 6.0 % | T6 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar | A50 | ||
6.0 % Show Material materials with Elongation of 6.0 % | T6 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | A100 | ||
7.0 % Show Material materials with Elongation of 7.0 % | T6 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | A50 | ||
7.0 % Show Material materials with Elongation of 7.0 % | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | A100 | ||
8.0 % Show Material materials with Elongation of 8.0 % | T6 | EN 573-3, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar | A100 | ||
20.0 °C | 2.0 % Show Material materials with Elongation of 2.0 % | T6 | EN 573-3 | Flat | Transverse | |
20.0 °C | 2.0 % Show Material materials with Elongation of 2.0 % | T6 | EN 573-3 | Sheet | ||
20.0 °C | 3.0 % Show Material materials with Elongation of 3.0 % | T6 | EN 573-3 | Forging | Transverse | |
20.0 °C | 3.0 % Show Material materials with Elongation of 3.0 % | T6 | EN 573-3 | Forging | ||
20.0 °C | 4.0 % Show Material materials with Elongation of 4.0 % | T6 | EN 573-3 | Flat | Transverse | |
20.0 °C | 4.0 % Show Material materials with Elongation of 4.0 % | T6 | EN 573-3 | Sheet, Flat | ||
20.0 °C | 4.0 % Show Material materials with Elongation of 4.0 % | T6 | EN 573-3 | Tube | A50 | |
20.0 °C | 5.0 % Show Material materials with Elongation of 5.0 % | T6 | EN 573-3 | Flat | Transverse | |
20.0 °C | 5.0 % Show Material materials with Elongation of 5.0 % | T6 | EN 573-3 | Rod, Sheet, Flat | ||
20.0 °C | 5.0 % Show Material materials with Elongation of 5.0 % | T6 | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 6.0 % Show Material materials with Elongation of 6.0 % | T6 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 6.0 % Show Material materials with Elongation of 6.0 % | T6 | EN 573-3 | Flat | Transverse | |
20.0 °C | 6.0 % Show Material materials with Elongation of 6.0 % | T6 | EN 573-3 | Flat, Forging, Rod, Tube | ||
20.0 °C | 6.0 % Show Material materials with Elongation of 6.0 % | T6 | EN 573-3 | Rod, Tube, Flat | A50 | |
20.0 °C | 7.0 % Show Material materials with Elongation of 7.0 % | T6 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 7.0 % Show Material materials with Elongation of 7.0 % | T6 | EN 573-3 | Profile, Rod, Tube | ||
20.0 °C | 7.0 % Show Material materials with Elongation of 7.0 % | T6 | EN 573-3 | Flat | A50 | |
20.0 °C | 8.0 % Show Material materials with Elongation of 8.0 % | T6 | EN 573-3 | Rod, Tube | ||
20.0 °C | 8.0 % Show Material materials with Elongation of 8.0 % | T6 | EN 573-3 | Flat | A50 | |
20.0 °C | 13.0 % Show Material materials with Elongation of 13.0 % | T6 | EN 573-3 | A50 Transverse | ||
20.0 °C | 16.0 % Show Material materials with Elongation of 16.0 % | T6 | EN 573-3 | A50 Transverse | ||
Hardness, Brinell | 123.0 [-] Show Material materials with Hardness, Brinell of 123.0 [-] | T6 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
125.0 [-] Show Material materials with Hardness, Brinell of 125.0 [-] | T6 | EN 573-3, EN 586 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
126.0 [-] Show Material materials with Hardness, Brinell of 126.0 [-] | T6 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
131.0 [-] Show Material materials with Hardness, Brinell of 131.0 [-] | T6 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
133.0 [-] Show Material materials with Hardness, Brinell of 133.0 [-] | T6 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
135.0 [-] Show Material materials with Hardness, Brinell of 135.0 [-] | T6 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
138.0 [-] Show Material materials with Hardness, Brinell of 138.0 [-] | T6 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
20.0 °C | 123.0 - 133.0 [-] Show Material materials with Hardness, Brinell of 123.0 - 133.0 [-] | T6 | EN 573-3 | Flat | ||
20.0 °C | 123.0 - 135.0 [-] Show Material materials with Hardness, Brinell of 123.0 - 135.0 [-] | T6 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 123.0 - 138.0 [-] Show Material materials with Hardness, Brinell of 123.0 - 138.0 [-] | T6 | EN 573-3 | Flat | ||
20.0 °C | 123.0 - 131.0 [-] Show Material materials with Hardness, Brinell of 123.0 - 131.0 [-] | T6 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 123.0 - 126.0 [-] Show Material materials with Hardness, Brinell of 123.0 - 126.0 [-] | T6 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 123.0 [-] Show Material materials with Hardness, Brinell of 123.0 [-] | T6 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 125.0 [-] Show Material materials with Hardness, Brinell of 125.0 [-] | T6 | EN 573-3 | Forging | ||
20.0 °C | 126.0 - 133.0 [-] Show Material materials with Hardness, Brinell of 126.0 - 133.0 [-] | T6 | EN 573-3 | Flat | ||
20.0 °C | 126.0 - 135.0 [-] Show Material materials with Hardness, Brinell of 126.0 - 135.0 [-] | T6 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 126.0 - 138.0 [-] Show Material materials with Hardness, Brinell of 126.0 - 138.0 [-] | T6 | EN 573-3 | Flat | ||
20.0 °C | 126.0 - 131.0 [-] Show Material materials with Hardness, Brinell of 126.0 - 131.0 [-] | T6 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 126.0 [-] Show Material materials with Hardness, Brinell of 126.0 [-] | T6 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 131.0 - 133.0 [-] Show Material materials with Hardness, Brinell of 131.0 - 133.0 [-] | T6 | EN 573-3 | Flat | ||
20.0 °C | 131.0 - 135.0 [-] Show Material materials with Hardness, Brinell of 131.0 - 135.0 [-] | T6 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 131.0 - 138.0 [-] Show Material materials with Hardness, Brinell of 131.0 - 138.0 [-] | T6 | EN 573-3 | Flat | ||
20.0 °C | 131.0 [-] Show Material materials with Hardness, Brinell of 131.0 [-] | T6 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 133.0 [-] Show Material materials with Hardness, Brinell of 133.0 [-] | T6 | EN 573-3 | Flat | ||
20.0 °C | 133.0 - 135.0 [-] Show Material materials with Hardness, Brinell of 133.0 - 135.0 [-] | T6 | EN 573-3 | Flat | ||
20.0 °C | 133.0 - 138.0 [-] Show Material materials with Hardness, Brinell of 133.0 - 138.0 [-] | T6 | EN 573-3 | Flat | ||
20.0 °C | 135.0 [-] Show Material materials with Hardness, Brinell of 135.0 [-] | T6 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 135.0 - 138.0 [-] Show Material materials with Hardness, Brinell of 135.0 - 138.0 [-] | T6 | EN 573-3 | Flat | ||
20.0 °C | 138.0 [-] Show Material materials with Hardness, Brinell of 138.0 [-] | T6 | EN 573-3 | Flat | ||
20.0 °C | 140.0 [-] Show Material materials with Hardness, Brinell of 140.0 [-] | T6 | EN 573-3 | Profile, Rod, Tube | ||
20.0 °C | 150.0 [-] Show Material materials with Hardness, Brinell of 150.0 [-] | T6 | EN 573-3 | Flat | ||
Plane-Strain Fracture Toughnes | 20.0 °C | 18.3 - 30.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 18.3 - 30.6 MPa·√m | T6 | EN 573-3 | ||
20.0 °C | 18.3 - 19.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 18.3 - 19.1 MPa·√m | T6 | EN 573-3 | |||
20.0 °C | 18.3 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 18.3 MPa·√m | T6 | EN 573-3 | |||
20.0 °C | 19.1 - 30.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 19.1 - 30.6 MPa·√m | T6 | EN 573-3 | |||
20.0 °C | 19.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 19.1 MPa·√m | T6 | EN 573-3 | |||
20.0 °C | 30.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.6 MPa·√m | T6 | EN 573-3 | |||
Poisson's ratio | -269.0 °C | 0.335 [-] Show Material materials with Poisson's ratio of 0.335 [-] | T6 | EN 573-3 | ||
-195.0 °C | 0.337 [-] Show Material materials with Poisson's ratio of 0.337 [-] | T6 | EN 573-3 | |||
27.0 °C | 0.321 [-] Show Material materials with Poisson's ratio of 0.321 [-] | T6 | EN 573-3 | |||
Shear modulus | 27.4 GPa Show Material materials with Shear modulus of 27.4 GPa | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
Tensile strength | -269.0 °C | 817.0 MPa Show Material materials with Tensile strength of 817.0 MPa | T6 | EN 573-3 | ||
-195.0 °C | 593.6 MPa Show Material materials with Tensile strength of 593.6 MPa | T6 | EN 573-3 | |||
390.0 MPa Show Material materials with Tensile strength of 390.0 MPa | T6 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
410.0 MPa Show Material materials with Tensile strength of 410.0 MPa | T6 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
415.0 MPa Show Material materials with Tensile strength of 415.0 MPa | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
420.0 MPa Show Material materials with Tensile strength of 420.0 MPa | T6 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
430.0 MPa Show Material materials with Tensile strength of 430.0 MPa | T6 | EN 573-3, EN 586, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
435.0 MPa Show Material materials with Tensile strength of 435.0 MPa | T6 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
440.0 MPa Show Material materials with Tensile strength of 440.0 MPa | T6 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
450.0 MPa Show Material materials with Tensile strength of 450.0 MPa | T6 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
460.0 MPa Show Material materials with Tensile strength of 460.0 MPa | T6 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
465.0 MPa Show Material materials with Tensile strength of 465.0 MPa | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
20.0 °C | 220.0 MPa Show Material materials with Tensile strength of 220.0 MPa | T6 | EN 573-3 | Transverse | ||
20.0 °C | 390.0 MPa Show Material materials with Tensile strength of 390.0 MPa | T6 | EN 573-3 | Flat | Transverse | |
20.0 °C | 390.0 MPa Show Material materials with Tensile strength of 390.0 MPa | T6 | EN 573-3 | Sheet | ||
20.0 °C | 410.0 MPa Show Material materials with Tensile strength of 410.0 MPa | T6 | EN 573-3 | Flat | Transverse | |
20.0 °C | 410.0 MPa Show Material materials with Tensile strength of 410.0 MPa | T6 | EN 573-3 | Sheet, Flat | ||
20.0 °C | 415.0 MPa Show Material materials with Tensile strength of 415.0 MPa | T6 | EN 573-3 | Rod, Tube, Profile | ||
20.0 °C | 420.0 MPa Show Material materials with Tensile strength of 420.0 MPa | T6 | EN 573-3 | Flat | Transverse | |
20.0 °C | 420.0 MPa Show Material materials with Tensile strength of 420.0 MPa | T6 | EN 573-3 | Rod, Sheet, Flat | ||
20.0 °C | 430.0 MPa Show Material materials with Tensile strength of 430.0 MPa | T6 | EN 573-3 | Forging | Transverse | |
20.0 °C | 430.0 MPa Show Material materials with Tensile strength of 430.0 MPa | T6 | EN 573-3 | Rod, Forging, Flat | ||
20.0 °C | 435.0 MPa Show Material materials with Tensile strength of 435.0 MPa | T6 | EN 573-3 | Flat | Transverse | |
20.0 °C | 435.0 MPa Show Material materials with Tensile strength of 435.0 MPa | T6 | EN 573-3 | Sheet | ||
20.0 °C | 440.0 MPa Show Material materials with Tensile strength of 440.0 MPa | T6 | EN 573-3 | Flat | Transverse | |
20.0 °C | 440.0 MPa Show Material materials with Tensile strength of 440.0 MPa | T6 | EN 573-3 | Forging, Flat | ||
20.0 °C | 450.0 MPa Show Material materials with Tensile strength of 450.0 MPa | T6 | EN 573-3 | Flat | Transverse | |
20.0 °C | 450.0 MPa Show Material materials with Tensile strength of 450.0 MPa | T6 | EN 573-3 | Rod, Tube, Sheet, Flat | ||
20.0 °C | 460.0 MPa Show Material materials with Tensile strength of 460.0 MPa | T6 | EN 573-3 | Flat | Transverse | |
20.0 °C | 460.0 MPa Show Material materials with Tensile strength of 460.0 MPa | T6 | EN 573-3 | Rod, Profile, Flat | ||
20.0 °C | 465.0 MPa Show Material materials with Tensile strength of 465.0 MPa | T6 | EN 573-3 | Rod | ||
27.0 °C | 534.3 MPa Show Material materials with Tensile strength of 534.3 MPa | T6 | EN 573-3 | |||
Yield strength | -269.0 °C | 706.7 MPa Show Material materials with Yield strength of 706.7 MPa | T6 | EN 573-3 | RP02 | |
-195.0 °C | 520.6 MPa Show Material materials with Yield strength of 520.6 MPa | T6 | EN 573-3 | RP02 | ||
320.0 MPa Show Material materials with Yield strength of 320.0 MPa | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | RP02 | ||
340.0 MPa Show Material materials with Yield strength of 340.0 MPa | T6 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | RP02 | ||
350.0 MPa Show Material materials with Yield strength of 350.0 MPa | T6 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | RP02 | ||
360.0 MPa Show Material materials with Yield strength of 360.0 MPa | T6 | EN 573-3, EN 485, EN 586 | Strip, Sheet, Plate, Forging, Tube, Bar | RP02 | ||
370.0 MPa Show Material materials with Yield strength of 370.0 MPa | T6 | EN 573-3, EN 586, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | RP02 | ||
380.0 MPa Show Material materials with Yield strength of 380.0 MPa | T6 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar | RP02 | ||
390.0 MPa Show Material materials with Yield strength of 390.0 MPa | T6 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | RP02 | ||
395.0 MPa Show Material materials with Yield strength of 395.0 MPa | T6 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | RP02 | ||
400.0 MPa Show Material materials with Yield strength of 400.0 MPa | T6 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | RP02 | ||
415.0 MPa Show Material materials with Yield strength of 415.0 MPa | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | RP02 | ||
420.0 MPa Show Material materials with Yield strength of 420.0 MPa | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | RP02 | ||
20.0 °C | 25.0 MPa Show Material materials with Yield strength of 25.0 MPa | T6 | EN 573-3 | Rod | RP02 | |
20.0 °C | 75.0 MPa Show Material materials with Yield strength of 75.0 MPa | T6 | EN 573-3 | Rod | RP02 | |
20.0 °C | 140.0 MPa Show Material materials with Yield strength of 140.0 MPa | T6 | EN 573-3 | RP02 Transverse | ||
20.0 °C | 150.0 MPa Show Material materials with Yield strength of 150.0 MPa | T6 | EN 573-3 | Rod | RP02 | |
20.0 °C | 200.0 MPa Show Material materials with Yield strength of 200.0 MPa | T6 | EN 573-3 | Rod | RP02 | |
20.0 °C | 250.0 MPa Show Material materials with Yield strength of 250.0 MPa | T6 | EN 573-3 | Rod | RP02 | |
20.0 °C | 320.0 MPa Show Material materials with Yield strength of 320.0 MPa | T6 | EN 573-3 | Rod | RP02 | |
20.0 °C | 340.0 MPa Show Material materials with Yield strength of 340.0 MPa | T6 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 340.0 MPa Show Material materials with Yield strength of 340.0 MPa | T6 | EN 573-3 | Sheet | RP02 | |
20.0 °C | 350.0 MPa Show Material materials with Yield strength of 350.0 MPa | T6 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 350.0 MPa Show Material materials with Yield strength of 350.0 MPa | T6 | EN 573-3 | Rod, Sheet, Flat | RP02 | |
20.0 °C | 360.0 MPa Show Material materials with Yield strength of 360.0 MPa | T6 | EN 573-3 | Forging, Flat | RP02 Transverse | |
20.0 °C | 360.0 MPa Show Material materials with Yield strength of 360.0 MPa | T6 | EN 573-3 | Forging, Sheet | RP02 | |
20.0 °C | 360.0 - 385.0 MPa Show Material materials with Yield strength of 360.0 - 385.0 MPa | T6 | EN 573-3 | |||
20.0 °C | 370.0 MPa Show Material materials with Yield strength of 370.0 MPa | T6 | EN 573-3 | Forging | RP02 Transverse | |
20.0 °C | 370.0 MPa Show Material materials with Yield strength of 370.0 MPa | T6 | EN 573-3 | Rod, Tube, Forging, Profile, Flat | RP02 | |
20.0 °C | 380.0 MPa Show Material materials with Yield strength of 380.0 MPa | T6 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 380.0 MPa Show Material materials with Yield strength of 380.0 MPa | T6 | EN 573-3 | Rod, Tube, Forging, Sheet, Flat | RP02 | |
20.0 °C | 390.0 MPa Show Material materials with Yield strength of 390.0 MPa | T6 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 390.0 MPa Show Material materials with Yield strength of 390.0 MPa | T6 | EN 573-3 | Sheet, Flat | RP02 | |
20.0 °C | 395.0 MPa Show Material materials with Yield strength of 395.0 MPa | T6 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 395.0 MPa Show Material materials with Yield strength of 395.0 MPa | T6 | EN 573-3 | Flat | RP02 | |
20.0 °C | 400.0 MPa Show Material materials with Yield strength of 400.0 MPa | T6 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 400.0 MPa Show Material materials with Yield strength of 400.0 MPa | T6 | EN 573-3 | Tube, Flat | RP02 | |
20.0 °C | 410.0 MPa Show Material materials with Yield strength of 410.0 MPa | T6 | EN 573-3 | Flat | RP02 | |
20.0 °C | 415.0 MPa Show Material materials with Yield strength of 415.0 MPa | T6 | EN 573-3 | Rod, Profile | RP02 | |
20.0 °C | 420.0 MPa Show Material materials with Yield strength of 420.0 MPa | T6 | EN 573-3 | Rod | RP02 | |
27.0 °C | 485.4 MPa Show Material materials with Yield strength of 485.4 MPa | T6 | EN 573-3 | RP02 |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | -50 °C | 2.1e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | |
-50.0 °C | 2.1e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | ||
20 °C | 2.1e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | ||
20 °C | 2.28e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.28e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | ||
20 °C | 2.3e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
20 °C | 2.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | ||
20 °C | 2.46e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.46e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | ||
100 °C | 2.28e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.28e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | ||
100.0 °C | 2.28e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.28e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | ||
100 °C | 2.3e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
200 °C | 2.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | ||
200.0 °C | 2.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | ||
300 °C | 2.46e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.46e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | ||
300.0 °C | 2.46e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.46e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | ||
Melting point | 505.0 - 635.0 °C Show Material materials with Melting point of 505.0 - 635.0 °C | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
510.0 - 640.0 °C Show Material materials with Melting point of 510.0 - 640.0 °C | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
Specific heat capacity | 816.0 - 963.0 J/(kg·K) Show Material materials with Specific heat capacity of 816.0 - 963.0 J/(kg·K) | Typical for Wrought 2000 Series Aluminium | ||||
Thermal conductivity | 134.0 - 193.0 W/(m·K) Show Material materials with Thermal conductivity of 134.0 - 193.0 W/(m·K) | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
20.0 °C | 140.0 - 200.0 W/(m·K) Show Material materials with Thermal conductivity of 140.0 - 200.0 W/(m·K) | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Forging, Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Bar |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 21000000.0 - 24000000.0 S/m Show Material materials with Electrical conductivity of 21000000.0 - 24000000.0 S/m | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |
20.0 °C | 20000000.0 - 29000000.0 S/m Show Material materials with Electrical conductivity of 20000000.0 - 29000000.0 S/m | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Forging, Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Bar | |
Electrical resistivity | 3.45e-08 - 5e-08 Ω·m Show Material materials with Electrical resistivity of 3.45e-08 - 5e-08 Ω·m | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |
4.17e-08 - 4.76e-08 Ω·m Show Material materials with Electrical resistivity of 4.17e-08 - 4.76e-08 Ω·m | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.1 % Show Material materials with Chromium of 0.1 % | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Forging, Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Bar |
Copper | 3.9 - 5.0 % Show Material materials with Copper of 3.9 - 5.0 % | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Forging, Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Bar |
Iron | 0.5 % Show Material materials with Iron of 0.5 % | T6 | EN 573-3 | Profile, Rod, Flat, Tube |
0.7 % Show Material materials with Iron of 0.7 % | T6 | EN 573-3 | Forging, Profile, Rod, Flat, Tube, Sheet | |
0.70 % Show Material materials with Iron of 0.70 % | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |
Magnesium | 0.2 - 0.8 % Show Material materials with Magnesium of 0.2 - 0.8 % | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Forging, Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Bar |
Manganese | 0.4 - 1.2 % Show Material materials with Manganese of 0.4 - 1.2 % | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Forging, Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Bar |
Nickel | 0.1 Show Material materials with Nickel of 0.1 | T6 | EN 573-3 | Profile, Rod, Flat, Tube |
Silicon | 0.5 - 1.2 % Show Material materials with Silicon of 0.5 - 1.2 % | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Forging, Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Bar |
0.5 - 0.9 % Show Material materials with Silicon of 0.5 - 0.9 % | T6 | EN 573-3 | Profile, Rod, Flat, Tube | |
Titanium | 0.15 % Show Material materials with Titanium of 0.15 % | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Forging, Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Bar |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | Forging, Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not suitable, Protective: acceptable | |
Brazing | hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable | |
Corrosion properties | Seawater: sufficient, weathering: acceptable | |
Workability | Bending / Spinning (cold): gut (O) / ungeeignet, Impact extrusion (cold): not suitable, Deep drawing / upsetting (Condition) acceptable (O) / not suitable |