EN 573-3 Grade AW-2024 T851

Want to keep this datasheet? Save it now in your required format

Description

Aluminum EN AW-2024, known for its use in aircraft industry, is an alloy that offers excellent strength. When in the annealed condition it is readily formed and has good machinability. Though it has a relatively low level of corrosion resistance, it can be machined to a high finish.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

20.0 °C

2.77 g/cm³

Show Material materials with Density of 2.77 g/cm³

T851

EN 573-3

Rod, Sheet, Flat

2.77 g/cm³

Show Material materials with Density of 2.77 g/cm³

T851

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending angle 90°

5.0 °/t

Show Material materials with Bending angle 90° of 5.0 °/t

T851

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

7.0 °/t

Show Material materials with Bending angle 90° of 7.0 °/t

T851

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Elastic modulus

20.0 °C

70.0 - 74.5 GPa

Show Material materials with Elastic modulus of 70.0 - 74.5 GPa

T851

EN 573-3

Rod, Sheet, Flat

73.0 GPa

Show Material materials with Elastic modulus of 73.0 GPa

T851

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Elongation

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

T851

EN 573-3

Sheet, Flat, Rod

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

T851

EN 573-3

Rod

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

T851

EN 573-3

Rod

A50

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

T851

EN 573-3

Rod

A50

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

T851

EN 573-3

Flat

A50

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

T851

EN 573-3

Flat

A50

5.0 %

Show Material materials with Elongation of 5.0 %

T851

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A50

6.0 %

Show Material materials with Elongation of 6.0 %

T851

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A50

4.0 %

Show Material materials with Elongation of 4.0 %

T851

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A50

2.0 %

Show Material materials with Elongation of 2.0 %

T851

EN 573-3, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A50

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T851

EN 573-3

Transverse

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

T851

EN 573-3

Transverse

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

T851

EN 573-3

Flat

Transverse

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

T851

EN 573-3

Sheet

A50 Transverse

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

T851

EN 573-3

Sheet

A50 Transverse

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

T851

EN 573-3

Flat

A50 Transverse

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

T851

EN 573-3

Flat

A50 Transverse

3.0 %

Show Material materials with Elongation of 3.0 %

T851

EN 573-3, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A100

Hardness, Brinell

20.0 °C

136.0 [-]

Show Material materials with Hardness, Brinell of 136.0 [-]

T851

EN 573-3

Sheet, Flat

20.0 °C

130.0 [-]

Show Material materials with Hardness, Brinell of 130.0 [-]

T851

EN 573-3

Rod

20.0 °C

138.0 [-]

Show Material materials with Hardness, Brinell of 138.0 [-]

T851

EN 573-3

Flat

20.0 °C

137.0 - 138.0 [-]

Show Material materials with Hardness, Brinell of 137.0 - 138.0 [-]

T851

EN 573-3

Flat

20.0 °C

137.0 [-]

Show Material materials with Hardness, Brinell of 137.0 [-]

T851

EN 573-3

Flat

20.0 °C

136.0 - 138.0 [-]

Show Material materials with Hardness, Brinell of 136.0 - 138.0 [-]

T851

EN 573-3

Flat

20.0 °C

136.0 - 137.0 [-]

Show Material materials with Hardness, Brinell of 136.0 - 137.0 [-]

T851

EN 573-3

Flat

138.0 [-]

Show Material materials with Hardness, Brinell of 138.0 [-]

T851

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

136.0 [-]

Show Material materials with Hardness, Brinell of 136.0 [-]

T851

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

137.0 [-]

Show Material materials with Hardness, Brinell of 137.0 [-]

T851

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Unlock all property charts

Plane-Strain Fracture Toughnes

20.0 °C

22.3 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.3 MPa·√m

T851

EN 573-3

-196.0 °C

24.4 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 24.4 MPa·√m

T851

EN 573-3

20.0 °C

24.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 24.0 MPa·√m

T851

EN 573-3

Sheet

20.0 °C

23.0 - 24.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 23.0 - 24.0 MPa·√m

T851

EN 573-3

Sheet

20.0 °C

18.0 - 24.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 18.0 - 24.0 MPa·√m

T851

EN 573-3

Sheet

20.0 °C

23.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 23.0 MPa·√m

T851

EN 573-3

Sheet

20.0 °C

18.0 - 23.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 18.0 - 23.0 MPa·√m

T851

EN 573-3

Sheet

20.0 °C

18.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 18.0 MPa·√m

T851

EN 573-3

Sheet

Unlock all property charts

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 2000 Series Aluminium

Shear modulus

20.0 °C

27.0 - 28.0 GPa

Show Material materials with Shear modulus of 27.0 - 28.0 GPa

T851

EN 573-3

Rod, Sheet, Flat

27.4 GPa

Show Material materials with Shear modulus of 27.4 GPa

T851

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Tensile strength

20.0 °C

455.0 MPa

Show Material materials with Tensile strength of 455.0 MPa

T851

EN 573-3

Sheet, Rod, Flat

20.0 °C

460.0 MPa

Show Material materials with Tensile strength of 460.0 MPa

T851

EN 573-3

Flat

460.0 MPa

Show Material materials with Tensile strength of 460.0 MPa

T851

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

455.0 MPa

Show Material materials with Tensile strength of 455.0 MPa

T851

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

420.0 MPa

Show Material materials with Tensile strength of 420.0 MPa

T851

EN 573-3

Transverse

20.0 °C

400.0 MPa

Show Material materials with Tensile strength of 400.0 MPa

T851

EN 573-3

Transverse

20.0 °C

425.0 MPa

Show Material materials with Tensile strength of 425.0 MPa

T851

EN 573-3

Sheet

Transverse

20.0 °C

460.0 MPa

Show Material materials with Tensile strength of 460.0 MPa

T851

EN 573-3

Flat

Transverse

20.0 °C

455.0 MPa

Show Material materials with Tensile strength of 455.0 MPa

T851

EN 573-3

Flat

Transverse

Unlock all property charts

Yield strength

20.0 °C

395.0 MPa

Show Material materials with Yield strength of 395.0 MPa

T851

EN 573-3

Sheet

RP02

20.0 °C

400.0 MPa

Show Material materials with Yield strength of 400.0 MPa

T851

EN 573-3

Rod, Flat

RP02

400.0 MPa

Show Material materials with Yield strength of 400.0 MPa

T851

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

RP02

395.0 MPa

Show Material materials with Yield strength of 395.0 MPa

T851

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

RP02

20.0 °C

290.0 MPa

Show Material materials with Yield strength of 290.0 MPa

T851

EN 573-3

RP02 Transverse

20.0 °C

285.0 MPa

Show Material materials with Yield strength of 285.0 MPa

T851

EN 573-3

RP02 Transverse

20.0 °C

275.0 MPa

Show Material materials with Yield strength of 275.0 MPa

T851

EN 573-3

Sheet

RP02 Transverse

20.0 °C

400.0 MPa

Show Material materials with Yield strength of 400.0 MPa

T851

EN 573-3

Flat

RP02 Transverse

20.0 °C

395.0 MPa

Show Material materials with Yield strength of 395.0 MPa

T851

EN 573-3

Flat

RP02 Transverse

20.0 °C, -196.0 °C

444.0 MPa

Show Material materials with Yield strength of 444.0 MPa

T851

EN 573-3

20.0 °C

455.0 MPa

Show Material materials with Yield strength of 455.0 MPa

T851

EN 573-3

Sheet

Unlock all property charts

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

300 °C, 20 °C

2.4699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4699999999999997e-05 1/K

T851

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

200 °C, 20 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

T851

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

100 °C, 20 °C

2.2899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2899999999999998e-05 1/K

T851

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20 °C, -50 °C

2.11e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.11e-05 1/K

T851

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

100 °C, 20 °C

2.3199999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K

T851

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Unlock all property charts

Melting point

505.0 - 640.0 °C

Show Material materials with Melting point of 505.0 - 640.0 °C

T851

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

505.0 - 635.0 °C

Show Material materials with Melting point of 505.0 - 635.0 °C

T851

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Specific heat capacity

20.0 °C

875.0 J/(kg·K)

Show Material materials with Specific heat capacity of 875.0 J/(kg·K)

T851

EN 573-3

Rod, Sheet, Flat

875.0 J/(kg·K)

Show Material materials with Specific heat capacity of 875.0 J/(kg·K)

T851

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Thermal conductivity

20.0 °C

130.0 - 150.0 W/(m·K)

Show Material materials with Thermal conductivity of 130.0 - 150.0 W/(m·K)

T851

EN 573-3, EN 485, EN 754

Rod, Sheet, Flat, Strip, Plate, Forging, Tube, Welded Tube, Bar

121.0 - 193.0 W/(m·K)

Show Material materials with Thermal conductivity of 121.0 - 193.0 W/(m·K)

T851

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

18000000.0 - 21000000.0 S/m

Show Material materials with Electrical conductivity of 18000000.0 - 21000000.0 S/m

T851

EN 573-3, EN 485, EN 754

Rod, Sheet, Flat, Strip, Plate, Forging, Tube, Welded Tube, Bar

17000000.0 - 29000000.0 S/m

Show Material materials with Electrical conductivity of 17000000.0 - 29000000.0 S/m

T851

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Electrical resistivity

4.76e-08 - 5.56e-08 Ω·m

Show Material materials with Electrical resistivity of 4.76e-08 - 5.56e-08 Ω·m

T851

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

3.45e-08 - 5.88e-08 Ω·m

Show Material materials with Electrical resistivity of 3.45e-08 - 5.88e-08 Ω·m

T851

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

T851

EN 573-3, EN 485, EN 754

Sheet, Flat, Rod, Strip, Plate, Forging, Tube, Welded Tube, Bar

Copper

3.8 - 4.9 %

Show Material materials with Copper of 3.8 - 4.9 %

T851

EN 573-3, EN 485, EN 754

Sheet, Flat, Rod, Strip, Plate, Forging, Tube, Welded Tube, Bar

Iron

0.5 %

Show Material materials with Iron of 0.5 %

T851

EN 573-3

Sheet, Flat, Rod

0.50 %

Show Material materials with Iron of 0.50 %

T851

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Magnesium

1.2 - 1.8 %

Show Material materials with Magnesium of 1.2 - 1.8 %

T851

EN 573-3, EN 485, EN 754

Sheet, Flat, Rod, Strip, Plate, Forging, Tube, Welded Tube, Bar

Manganese

0.3 - 0.9 %

Show Material materials with Manganese of 0.3 - 0.9 %

T851

EN 573-3, EN 485, EN 754

Sheet, Flat, Rod, Strip, Plate, Forging, Tube, Welded Tube, Bar

Silicon

0.5 %

Show Material materials with Silicon of 0.5 %

T851

EN 573-3, EN 485, EN 754

Sheet, Flat, Rod, Strip, Plate, Forging, Tube, Welded Tube, Bar

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

T851

EN 573-3, EN 485, EN 754

Sheet, Flat, Rod, Strip, Plate, Forging, Tube, Welded Tube, Bar

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

T851

EN 573-3, EN 485, EN 754

Sheet, Flat, Rod, Strip, Plate, Forging, Tube, Welded Tube, Bar

Technological properties

Property
Anodizing

decorative: not suitable, Protective: good

Brazing

hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable

Corrosion properties

Seawater: poor, weathering: poor

Workability

Bending / Spinning (cold): sufficient (O) / acceptable (O), Impact extrusion (cold): acceptable (O), Deep drawing / upsetting (Condition) acceptable (O) / sufficient (O)