General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Density | 2.77 g/cm³ Show Material materials with Density of 2.77 g/cm³ | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 70.0 - 73.0 GPa Show Material materials with Elastic modulus of 70.0 - 73.0 GPa | Typical for Wrought 2000 Series Aluminium | ||||
Elongation | 4.0 % Show Material materials with Elongation of 4.0 % | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate | A50 | |
5.0 % Show Material materials with Elongation of 5.0 % | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate | A50 | ||
6.0 % Show Material materials with Elongation of 6.0 % | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate | |||
7.0 % Show Material materials with Elongation of 7.0 % | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate | |||
20.0 °C | 4.0 % Show Material materials with Elongation of 4.0 % | T6 | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 5.0 % Show Material materials with Elongation of 5.0 % | T6 | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 6.0 % Show Material materials with Elongation of 6.0 % | T6 | EN 573-3 | Profile, Rod, Tube | ||
20.0 °C | 7.0 % Show Material materials with Elongation of 7.0 % | T6 | EN 573-3 | Profile, Rod, Tube | ||
Hardness, Brinell | 140.0 [-] Show Material materials with Hardness, Brinell of 140.0 [-] | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate | ||
145.0 [-] Show Material materials with Hardness, Brinell of 145.0 [-] | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate | |||
20.0 °C | 140.0 [-] Show Material materials with Hardness, Brinell of 140.0 [-] | T6 | EN 573-3 | Profile, Rod, Tube | ||
20.0 °C | 140.0 - 145.0 [-] Show Material materials with Hardness, Brinell of 140.0 - 145.0 [-] | T6 | EN 573-3 | Profile, Rod, Tube | ||
20.0 °C | 145.0 [-] Show Material materials with Hardness, Brinell of 145.0 [-] | T6 | EN 573-3 | Profile, Rod, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Shear modulus | 26.0 - 27.5 GPa Show Material materials with Shear modulus of 26.0 - 27.5 GPa | Typical for Wrought 2000 Series Aluminium | ||||
Tensile strength | 410.0 MPa Show Material materials with Tensile strength of 410.0 MPa | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate | ||
420.0 MPa Show Material materials with Tensile strength of 420.0 MPa | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate | |||
20.0 °C | 410.0 MPa Show Material materials with Tensile strength of 410.0 MPa | T6 | EN 573-3 | Profile, Rod, Tube | ||
20.0 °C | 420.0 MPa Show Material materials with Tensile strength of 420.0 MPa | T6 | EN 573-3 | Profile, Rod, Tube |
Thermal
Property | Value | Comment |
---|---|---|
Coefficient of thermal expansion | 1.6e-05 - 2.4e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.6e-05 - 2.4e-05 1/K | Typical for Wrought 2000 Series Aluminium |
Melting point | 500.0 - 650.0 °C Show Material materials with Melting point of 500.0 - 650.0 °C | Typical for Wrought 2000 Series Aluminium |
Specific heat capacity | 816.0 - 963.0 J/(kg·K) Show Material materials with Specific heat capacity of 816.0 - 963.0 J/(kg·K) | Typical for Wrought 2000 Series Aluminium |
Thermal conductivity | 112.0 - 251.0 W/(m·K) Show Material materials with Thermal conductivity of 112.0 - 251.0 W/(m·K) | Typical for Wrought 2000 Series Aluminium |
Electrical
Property | Value | Comment |
---|---|---|
Electrical conductivity | 18000000.0 - 30000000.0 S/m Show Material materials with Electrical conductivity of 18000000.0 - 30000000.0 S/m | Typical for Wrought 2000 Series Aluminium |
Electrical resistivity | 3.4e-08 - 6e-08 Ω·m Show Material materials with Electrical resistivity of 3.4e-08 - 6e-08 Ω·m | Typical for Wrought 2000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Copper | 1.8 - 2.7 % Show Material materials with Copper of 1.8 - 2.7 % | T6 | EN 573-3, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate |
Iron | 0.9 - 1.4 % Show Material materials with Iron of 0.9 - 1.4 % | T6 | EN 573-3, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate |
Magnesium | 1.2 - 1.8 % Show Material materials with Magnesium of 1.2 - 1.8 % | T6 | EN 573-3, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate |
Manganese | 0.25 % Show Material materials with Manganese of 0.25 % | T6 | EN 573-3, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate |
Nickel | 0.8 - 1.4 % Show Material materials with Nickel of 0.8 - 1.4 % | T6 | EN 573-3, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate |
Silicon | 0.15 - 0.25 % Show Material materials with Silicon of 0.15 - 0.25 % | T6 | EN 573-3, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate |
Titanium | 0.2 % Show Material materials with Titanium of 0.2 % | T6 | EN 573-3, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate |
Zinc | 0.15 % Show Material materials with Zinc of 0.15 % | T6 | EN 573-3, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate |
Technological properties
Property | ||
---|---|---|
Workability | Moderate Workability |