Naturally hard AlFeMn alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,Aludium,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated StandardsShape

Density

2.74 g/cm³

Show Material materials with Density of 2.74 g/cm³

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2

Coil, Foil

2.74 g/cm³

Show Material materials with Density of 2.74 g/cm³

O

EN 573-3, EN 546, EN 683, EN 1396

Strip, Sheet

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.06 mm

Show Material materials with Thickness of 0.06 mm

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2

0.06 mm

Coil, Foil

0.2 mm

Show Material materials with Thickness of 0.2 mm

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2

0.2 mm

Coil, Foil

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2

Coil, Foil

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 8000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 8000 Series Aluminium

Shear modulus

25.0 GPa

Show Material materials with Shear modulus of 25.0 GPa

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2

Coil, Foil

Tensile strength

70.0 MPa

Show Material materials with Tensile strength of 70.0 MPa

O

EN 573-3, EN 1396

Strip, Sheet

20.0 °C

70.0 MPa

Show Material materials with Tensile strength of 70.0 MPa

O

EN 573-3

Sheet, Strip

Transverse

20.0 °C

80.0 - 135.0 MPa

Show Material materials with Tensile strength of 80.0 - 135.0 MPa

O

EN 573-3, EN 546

Strip, Sheet, Foil

20.0 °C

80.0 - 140.0 MPa

Show Material materials with Tensile strength of 80.0 - 140.0 MPa

O

EN 573-3

Foil

20.0 °C

85.0 - 140.0 MPa

Show Material materials with Tensile strength of 85.0 - 140.0 MPa

O

EN 573-3, EN 546

Strip, Sheet, Foil

20.0 °C

85.0 - 135.0 MPa

Show Material materials with Tensile strength of 85.0 - 135.0 MPa

O

EN 573-3

Foil

20.0 °C

90.0 - 140.0 MPa

Show Material materials with Tensile strength of 90.0 - 140.0 MPa

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2, EN 573-3, EN 546, EN 683

Coil, Foil, Strip, Sheet, Foil

20.0 °C

90.0 - 135.0 MPa

Show Material materials with Tensile strength of 90.0 - 135.0 MPa

O

EN 573-3

Foil

Yield strength

45.0 MPa

Show Material materials with Yield strength of 45.0 MPa

O

EN 573-3, EN 1396

Strip, Sheet

RP02

100.0 MPa

Show Material materials with Yield strength of 100.0 MPa

O

EN 573-3, EN 683

Strip, Sheet

RP02

100 MPa

Show Material materials with Yield strength of 100 MPa

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2

Coil, Foil

20.0 °C

45.0 MPa

Show Material materials with Yield strength of 45.0 MPa

O

EN 573-3

Sheet, Strip

RP02 Transverse

20.0 °C

70.0 MPa

Show Material materials with Yield strength of 70.0 MPa

O

EN 573-3

Foil

RP02

20.0 °C

95.0 MPa

Show Material materials with Yield strength of 95.0 MPa

O

EN 573-3

Foil

RP02

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2

Coil, Foil

20-100°C

Melting point

645.0 - 655.0 °C

Show Material materials with Melting point of 645.0 - 655.0 °C

Typical for Wrought 8000 Series Aluminium

Specific heat capacity

920.0 J/(kg·K)

Show Material materials with Specific heat capacity of 920.0 J/(kg·K)

Typical for Wrought 8000 Series Aluminium

Thermal conductivity

190.0 - 210.0 W/(m·K)

Show Material materials with Thermal conductivity of 190.0 - 210.0 W/(m·K)

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2

Coil, Foil

Electrical

PropertyValueConditionRelated StandardsShapeComment

Electrical conductivity

28000000.0 - 35000000.0 S/m

Show Material materials with Electrical conductivity of 28000000.0 - 35000000.0 S/m

Typical for Wrought 8000 Series Aluminium

Electrical resistivity

3.1e-08 Ω·m

Show Material materials with Electrical resistivity of 3.1e-08 Ω·m

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2

Coil, Foil

Chemical properties

PropertyValueConditionRelated StandardsShape

Copper

0.3 %

Show Material materials with Copper of 0.3 %

O

EN 573-3, EN 546, EN 683, EN 1396

Sheet, Strip, Foil

0.3 %

Show Material materials with Copper of 0.3 %

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2

Coil, Foil

Iron

1.2 - 2.0 %

Show Material materials with Iron of 1.2 - 2.0 %

O

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2, EN 546, EN 683, EN 1396

Sheet, Strip, Foil, Coil, Foil

Magnesium

0.1 %

Show Material materials with Magnesium of 0.1 %

O

EN 573-3, EN 546, EN 683, EN 1396

Sheet, Strip, Foil

0.1 %

Show Material materials with Magnesium of 0.1 %

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2

Coil, Foil

Manganese

0.3 - 1.0 %

Show Material materials with Manganese of 0.3 - 1.0 %

O

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2, EN 546, EN 683, EN 1396

Sheet, Strip, Foil, Coil, Foil

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

O

EN 573-3, EN 546, EN 683, EN 1396

Sheet, Strip, Foil

0.4 %

Show Material materials with Silicon of 0.4 %

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2

Coil, Foil

Zinc

0.1 %

Show Material materials with Zinc of 0.1 %

O

EN 573-3, EN 546, EN 683, EN 1396

Sheet, Strip, Foil

0.1 %

Show Material materials with Zinc of 0.1 %

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2

Coil, Foil

Technological properties

Property
Anodizing

Limited

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels; Roofing: Foil for bituminous coating; Doors: Sheets for composites/ sandwich Panels; Electronic devices: Housing of devices; Heat exchangers: Fins, Heat exchangers, General applications; Tubes: Industrial tubes, Flexible tubes, Pipes; Insulation; Semi-rigid and corrugated: Pet food, Smooth wall; Components: Automotive fins, Heat exchangers

Corrosion properties

Limited

Welding

Good

Workability

Very Good