EN 573-3 Grade AW-8011A H14

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlFeSi alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

H14

EN 573-3, EN 485, EN 541, EN 683

Strip, Sheet, Plate, Foil

20.0 °C

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

H14

EN 573-3

Sheet, Flat, Foil

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H14

EN 573-3, EN 485, EN 541, EN 683

Strip, Sheet, Plate, Foil

Hardness, Brinell

41.0 [-]

Show Material materials with Hardness, Brinell of 41.0 [-]

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Foil

20.0 °C

41.0 [-]

Show Material materials with Hardness, Brinell of 41.0 [-]

H14

EN 573-3

Flat

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 8000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 8000 Series Aluminium

Tensile strength

20.0 °C

110.0 - 165.0 MPa

Show Material materials with Tensile strength of 110.0 - 165.0 MPa

H14

EN 573-3

Sheet

20.0 °C

110.0 - 150.0 MPa

Show Material materials with Tensile strength of 110.0 - 150.0 MPa

H14

EN 573-3

Sheet

20.0 °C

120.0 - 170.0 MPa

Show Material materials with Tensile strength of 120.0 - 170.0 MPa

H14

EN 573-3, EN 683

Foil, Strip, Sheet, Plate

20.0 °C

125.0 - 165.0 MPa

Show Material materials with Tensile strength of 125.0 - 165.0 MPa

H14

EN 573-3, EN 485, EN 541

Sheet, Flat, Strip, Plate, Foil

20.0 °C

125.0 - 150.0 MPa

Show Material materials with Tensile strength of 125.0 - 150.0 MPa

H14

EN 573-3

Sheet

20.0 °C

125.0 - 170.0 MPa

Show Material materials with Tensile strength of 125.0 - 170.0 MPa

H14

EN 573-3

Flat

20.0 °C

125.0 - 170.0 MPa

Show Material materials with Tensile strength of 125.0 - 170.0 MPa

H14

EN 573-3

Flat

Transverse

20.0 °C

125.0 - 165.0 MPa

Show Material materials with Tensile strength of 125.0 - 165.0 MPa

H14

EN 573-3

Flat

Transverse

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H14

EN 573-3, EN 485, EN 541, EN 683

Strip, Sheet, Plate, Foil

100 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H14

EN 573-3, EN 485, EN 541, EN 683

Strip, Sheet, Plate, Foil

Melting point

640.0 - 655.0 °C

Show Material materials with Melting point of 640.0 - 655.0 °C

H14

EN 573-3, EN 485, EN 541, EN 683

Strip, Sheet, Plate, Foil

Specific heat capacity

920.0 J/(kg·K)

Show Material materials with Specific heat capacity of 920.0 J/(kg·K)

Typical for Wrought 8000 Series Aluminium

Thermal conductivity

20.0 °C

210.0 - 220.0 W/(m·K)

Show Material materials with Thermal conductivity of 210.0 - 220.0 W/(m·K)

H14

EN 573-3, EN 485, EN 541, EN 683

Sheet, Flat, Foil, Strip, Plate

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

34000000.0 - 35000000.0 S/m

Show Material materials with Electrical conductivity of 34000000.0 - 35000000.0 S/m

H14

EN 573-3, EN 485, EN 541, EN 683

Sheet, Flat, Foil, Strip, Plate

Electrical resistivity

2.86e-08 - 2.94e-08 Ω·m

Show Material materials with Electrical resistivity of 2.86e-08 - 2.94e-08 Ω·m

H14

EN 573-3, EN 485, EN 541, EN 683

Strip, Sheet, Plate, Foil

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

H14

EN 573-3, EN 485, EN 541, EN 683

Sheet, Flat, Foil, Strip, Plate

Copper

0.1 %

Show Material materials with Copper of 0.1 %

H14

EN 573-3, EN 485, EN 541, EN 683

Sheet, Flat, Foil, Strip, Plate

Iron

0.5 - 1.0 %

Show Material materials with Iron of 0.5 - 1.0 %

H14

EN 573-3, EN 485, EN 541, EN 683

Sheet, Flat, Foil, Strip, Plate

Magnesium

0.1 %

Show Material materials with Magnesium of 0.1 %

H14

EN 573-3, EN 485, EN 541, EN 683

Sheet, Flat, Foil, Strip, Plate

Manganese

0.1 %

Show Material materials with Manganese of 0.1 %

H14

EN 573-3, EN 485, EN 541, EN 683

Sheet, Flat, Foil, Strip, Plate

Silicon

0.4 - 0.8 %

Show Material materials with Silicon of 0.4 - 0.8 %

H14

EN 573-3, EN 485, EN 541, EN 683

Sheet, Flat, Foil, Strip, Plate

Titanium

0.05 %

Show Material materials with Titanium of 0.05 %

H14

EN 573-3, EN 485, EN 541, EN 683

Sheet, Flat, Foil, Strip, Plate

Zinc

0.1 %

Show Material materials with Zinc of 0.1 %

H14

EN 573-3, EN 485, EN 541, EN 683

Sheet, Flat, Foil, Strip, Plate

Technological properties

Property
Anodizing

decorative: acceptable, Protective: very good

Brazing

hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good

Corrosion properties

Seawater: sufficient, weathering: acceptable

Workability

Bending / Spinning (cold): good / good, Impact extrusion (cold): good, Deep drawing / upsetting (Condition) good (H14) / good (H14)