EN 573-3 Grade AW-8011A O

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlFeSi alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,Aludium,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683

Strip, Sheet, Plate, Foil

20.0 °C

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

O

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 541, EN 546-2

Sheet, Strip, Foil, Flat, Coil, Sheet, Strip, Foil

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.08 mm

Show Material materials with Thickness of 0.08 mm

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 541, EN 546-2

0.08 mm

Coil, Sheet, Strip, Foil

0.2 mm

Show Material materials with Thickness of 0.2 mm

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 541, EN 546-2

0.2 mm

Coil, Sheet, Strip, Foil

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

68.6 GPa

Show Material materials with Elastic modulus of 68.6 GPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 541, EN 546-2

Coil, Sheet, Strip, Foil

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683

Strip, Sheet, Plate, Foil

Hardness, Brinell

25.0 [-]

Show Material materials with Hardness, Brinell of 25.0 [-]

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil

20.0 °C

25.0 [-]

Show Material materials with Hardness, Brinell of 25.0 [-]

O

EN 573-3

Flat

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 8000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 8000 Series Aluminium

Shear modulus

25.725 GPa

Show Material materials with Shear modulus of 25.725 GPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 541, EN 546-2

Coil, Sheet, Strip, Foil

Tensile strength

85.0 MPa

Show Material materials with Tensile strength of 85.0 MPa

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil

90.0 - 120.0 MPa

Show Material materials with Tensile strength of 90.0 - 120.0 MPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 541, EN 546-2

Coil, Sheet, Strip, Foil

according to EN 485-2

20.0 °C

50.0 - 110.0 MPa

Show Material materials with Tensile strength of 50.0 - 110.0 MPa

O

EN 573-3, EN 546

Strip, Sheet, Plate, Foil

20.0 °C

50.0 - 115.0 MPa

Show Material materials with Tensile strength of 50.0 - 115.0 MPa

O

EN 573-3

Foil

20.0 °C

50.0 - 120.0 MPa

Show Material materials with Tensile strength of 50.0 - 120.0 MPa

O

EN 573-3

Foil

20.0 °C

50.0 - 130.0 MPa

Show Material materials with Tensile strength of 50.0 - 130.0 MPa

O

EN 573-3

Foil

20.0 °C

55.0 - 115.0 MPa

Show Material materials with Tensile strength of 55.0 - 115.0 MPa

O

EN 573-3, EN 546

Strip, Sheet, Plate, Foil

20.0 °C

55.0 - 120.0 MPa

Show Material materials with Tensile strength of 55.0 - 120.0 MPa

O

EN 573-3, EN 546

Strip, Sheet, Plate, Foil

20.0 °C

55.0 - 110.0 MPa

Show Material materials with Tensile strength of 55.0 - 110.0 MPa

O

EN 573-3

Foil

20.0 °C

55.0 - 130.0 MPa

Show Material materials with Tensile strength of 55.0 - 130.0 MPa

O

EN 573-3

Foil

20.0 °C

65.0 - 130.0 MPa

Show Material materials with Tensile strength of 65.0 - 130.0 MPa

O

EN 573-3, EN 546, EN 683

Strip, Sheet, Plate, Foil

20.0 °C

65.0 - 110.0 MPa

Show Material materials with Tensile strength of 65.0 - 110.0 MPa

O

EN 573-3

Foil

20.0 °C

65.0 - 115.0 MPa

Show Material materials with Tensile strength of 65.0 - 115.0 MPa

O

EN 573-3

Foil

20.0 °C

65.0 - 120.0 MPa

Show Material materials with Tensile strength of 65.0 - 120.0 MPa

O

EN 573-3

Foil

20.0 °C

80.0 - 120.0 MPa

Show Material materials with Tensile strength of 80.0 - 120.0 MPa

O

EN 573-3

Sheet, Strip

Transverse

20.0 °C

80.0 - 120.0 MPa

Show Material materials with Tensile strength of 80.0 - 120.0 MPa

O

EN 573-3, EN 1396

Strip, Sheet, Plate, Foil

20.0 °C

85.0 - 130.0 MPa

Show Material materials with Tensile strength of 85.0 - 130.0 MPa

O

EN 573-3

Flat

Transverse

20.0 °C

85.0 - 130.0 MPa

Show Material materials with Tensile strength of 85.0 - 130.0 MPa

O

EN 573-3

Flat

Yield strength

30.0 MPa

Show Material materials with Yield strength of 30.0 MPa

O

EN 573-3, EN 1396, EN 485

Strip, Sheet, Plate, Foil

RP02

30.0 - 70.0 MPa

Show Material materials with Yield strength of 30.0 - 70.0 MPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 541, EN 546-2

Coil, Sheet, Strip, Foil

according to EN 485-2

70.0 MPa

Show Material materials with Yield strength of 70.0 MPa

O

EN 573-3, EN 683

Strip, Sheet, Plate, Foil

RP02

20.0 °C

30.0 MPa

Show Material materials with Yield strength of 30.0 MPa

O

EN 573-3

Sheet, Strip, Flat

RP02 Transverse

20.0 °C

30.0 MPa

Show Material materials with Yield strength of 30.0 MPa

O

EN 573-3

Sheet, Strip, Flat

RP02

20.0 °C

70.0 MPa

Show Material materials with Yield strength of 70.0 MPa

O

EN 573-3

Foil

RP02

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683

Strip, Sheet, Plate, Foil

100 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683

Strip, Sheet, Plate, Foil

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 541, EN 546-2

Coil, Sheet, Strip, Foil

20-100°C

Melting point

640.0 - 655.0 °C

Show Material materials with Melting point of 640.0 - 655.0 °C

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683

Strip, Sheet, Plate, Foil

Specific heat capacity

920.0 J/(kg·K)

Show Material materials with Specific heat capacity of 920.0 J/(kg·K)

Typical for Wrought 8000 Series Aluminium

Thermal conductivity

201 W/(m·K)

Show Material materials with Thermal conductivity of 201 W/(m·K)

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 541, EN 546-2

Coil, Sheet, Strip, Foil

20.0 °C

210.0 - 220.0 W/(m·K)

Show Material materials with Thermal conductivity of 210.0 - 220.0 W/(m·K)

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683

Sheet, Strip, Foil, Flat, Plate

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

34000000.0 - 35000000.0 S/m

Show Material materials with Electrical conductivity of 34000000.0 - 35000000.0 S/m

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683

Sheet, Strip, Foil, Flat, Plate

Electrical resistivity

2.86e-08 - 2.94e-08 Ω·m

Show Material materials with Electrical resistivity of 2.86e-08 - 2.94e-08 Ω·m

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683

Strip, Sheet, Plate, Foil

3e-08 - 3.5e-08 Ω·m

Show Material materials with Electrical resistivity of 3e-08 - 3.5e-08 Ω·m

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 541, EN 546-2

Coil, Sheet, Strip, Foil

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683

Sheet, Strip, Foil, Flat, Plate

0.1 %

Show Material materials with Chromium of 0.1 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 541, EN 546-2

Coil, Sheet, Strip, Foil

Copper

0.1 %

Show Material materials with Copper of 0.1 %

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683

Sheet, Strip, Foil, Flat, Plate

0.1 %

Show Material materials with Copper of 0.1 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 541, EN 546-2

Coil, Sheet, Strip, Foil

Iron

0.5 - 1.0 %

Show Material materials with Iron of 0.5 - 1.0 %

O

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 541, EN 546-2, EN 1396, EN 485, EN 546, EN 683

Sheet, Strip, Foil, Flat, Coil, Sheet, Strip, Foil, Plate

Magnesium

0.1 %

Show Material materials with Magnesium of 0.1 %

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683

Sheet, Strip, Foil, Flat, Plate

0.1 %

Show Material materials with Magnesium of 0.1 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 541, EN 546-2

Coil, Sheet, Strip, Foil

Manganese

0.1 %

Show Material materials with Manganese of 0.1 %

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683

Sheet, Strip, Foil, Flat, Plate

0.1 %

Show Material materials with Manganese of 0.1 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 541, EN 546-2

Coil, Sheet, Strip, Foil

Silicon

0.4 - 0.8 %

Show Material materials with Silicon of 0.4 - 0.8 %

O

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 541, EN 546-2, EN 1396, EN 485, EN 546, EN 683

Sheet, Strip, Foil, Flat, Coil, Sheet, Strip, Foil, Plate

Titanium

0.05 %

Show Material materials with Titanium of 0.05 %

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683

Sheet, Strip, Foil, Flat, Plate

0.05 %

Show Material materials with Titanium of 0.05 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 541, EN 546-2

Coil, Sheet, Strip, Foil

Zinc

0.1 %

Show Material materials with Zinc of 0.1 %

O

EN 573-3, EN 1396, EN 485, EN 546, EN 683

Sheet, Strip, Foil, Flat, Plate

0.1 %

Show Material materials with Zinc of 0.1 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 541, EN 546-2

Coil, Sheet, Strip, Foil

Technological properties

Property
Anodizing

Good

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Foil for bituminous coating; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Interiors and ceilings: Sheets for mechanized panels; Furniture, Plinths, Blinds: Intermediate transformation/interior use; Heat exchangers: Fins, General applications; Tubes: Flexible tube, Pipes; Insulation; Closures: Long cups, Short cups, Easy open; Cosmetic: Cosmetic pieces; Pharmacy: Pharma and para-pharma; Semi-rigid and corrugated: Pet food, Smooth wall; Foil stock: Foil app

Brazing

hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good

Corrosion properties

Moderated

Welding

Excellent

Workability

Excellent