EN 573-3 Grade AW-8021B O

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlFe alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,Aludium,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated StandardsShape

Density

2.72 g/cm³

Show Material materials with Density of 2.72 g/cm³

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2

Coil, Foil

2.72 g/cm³

Show Material materials with Density of 2.72 g/cm³

O

EN 573-3, EN 546

Foil

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.09 mm

Show Material materials with Thickness of 0.09 mm

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2

0.09 mm

Coil, Foil

0.14 mm

Show Material materials with Thickness of 0.14 mm

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2

0.14 mm

Coil, Foil

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

69.0 - 72.0 GPa

Show Material materials with Elastic modulus of 69.0 - 72.0 GPa

Typical for Wrought 8000 Series Aluminium

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 8000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 8000 Series Aluminium

Tensile strength

20.0 °C

75.0 - 110.0 MPa

Show Material materials with Tensile strength of 75.0 - 110.0 MPa

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 573-3, EN 546

Coil, Foil, Foil

20.0 °C

65.0 - 105.0 MPa

Show Material materials with Tensile strength of 65.0 - 105.0 MPa

O

EN 573-3, EN 546

Foil

20.0 °C

60.0 - 100.0 MPa

Show Material materials with Tensile strength of 60.0 - 100.0 MPa

O

EN 573-3, EN 546

Foil

20.0 °C

70.0 - 110.0 MPa

Show Material materials with Tensile strength of 70.0 - 110.0 MPa

O

EN 573-3, EN 546

Foil

20.0 °C

65.0 - 100.0 MPa

Show Material materials with Tensile strength of 65.0 - 100.0 MPa

O

EN 573-3

Foil

20.0 °C

70.0 - 100.0 MPa

Show Material materials with Tensile strength of 70.0 - 100.0 MPa

O

EN 573-3

Foil

20.0 °C

75.0 - 100.0 MPa

Show Material materials with Tensile strength of 75.0 - 100.0 MPa

O

EN 573-3

Foil

20.0 °C

60.0 - 105.0 MPa

Show Material materials with Tensile strength of 60.0 - 105.0 MPa

O

EN 573-3

Foil

20.0 °C

70.0 - 105.0 MPa

Show Material materials with Tensile strength of 70.0 - 105.0 MPa

O

EN 573-3

Foil

20.0 °C

75.0 - 105.0 MPa

Show Material materials with Tensile strength of 75.0 - 105.0 MPa

O

EN 573-3

Foil

20.0 °C

60.0 - 110.0 MPa

Show Material materials with Tensile strength of 60.0 - 110.0 MPa

O

EN 573-3

Foil

20.0 °C

65.0 - 110.0 MPa

Show Material materials with Tensile strength of 65.0 - 110.0 MPa

O

EN 573-3

Foil

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2

Coil, Foil

Melting point

645.0 - 655.0 °C

Show Material materials with Melting point of 645.0 - 655.0 °C

Typical for Wrought 8000 Series Aluminium

Specific heat capacity

920.0 J/(kg·K)

Show Material materials with Specific heat capacity of 920.0 J/(kg·K)

Typical for Wrought 8000 Series Aluminium

Thermal conductivity

167.0 - 220.0 W/(m·K)

Show Material materials with Thermal conductivity of 167.0 - 220.0 W/(m·K)

Typical for Wrought 8000 Series Aluminium

Electrical

PropertyValueComment

Electrical conductivity

28000000.0 - 35000000.0 S/m

Show Material materials with Electrical conductivity of 28000000.0 - 35000000.0 S/m

Typical for Wrought 8000 Series Aluminium

Electrical resistivity

2.8e-08 - 3.5e-08 Ω·m

Show Material materials with Electrical resistivity of 2.8e-08 - 3.5e-08 Ω·m

Typical for Wrought 8000 Series Aluminium

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.03 %

Show Material materials with Chromium of 0.03 %

O

EN 573-3, EN 546

Foil

0.03 %

Show Material materials with Chromium of 0.03 %

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2

Coil, Foil

Copper

0.05 %

Show Material materials with Copper of 0.05 %

O

EN 573-3, EN 546

Foil

0.05 %

Show Material materials with Copper of 0.05 %

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2

Coil, Foil

Iron

1.1 - 1.7 %

Show Material materials with Iron of 1.1 - 1.7 %

O

EN 573-3, EN 546, EN 573-1, EN 573-2, EN 573-3, EN 546-2

Foil, Coil, Foil

Magnesium

0.01 %

Show Material materials with Magnesium of 0.01 %

O

EN 573-3, EN 546

Foil

0.01 %

Show Material materials with Magnesium of 0.01 %

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2

Coil, Foil

Manganese

0.03 %

Show Material materials with Manganese of 0.03 %

O

EN 573-3, EN 546

Foil

0.03 %

Show Material materials with Manganese of 0.03 %

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2

Coil, Foil

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

O

EN 573-3, EN 546

Foil

0.4 %

Show Material materials with Silicon of 0.4 %

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2

Coil, Foil

Titanium

0.05 %

Show Material materials with Titanium of 0.05 %

O

EN 573-3, EN 546

Foil

0.05 %

Show Material materials with Titanium of 0.05 %

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2

Coil, Foil

Zinc

0.05 %

Show Material materials with Zinc of 0.05 %

O

EN 573-3, EN 546

Foil

0.05 %

Show Material materials with Zinc of 0.05 %

O

EN 573-1, EN 573-2, EN 573-3, EN 546-2

Coil, Foil

Technological properties

Property
Application areas

Foil stock: Foil app

Workability

Excellent